1 CAS Key Laboratory of Nuclear Materials and Safety Assessment, Institute of Metal Research, Chinese Academy of Sciences, Shenyang 110016, China 2 School of Materials Science and Engineering, University of Science and Technology of China, Shenyang 110016, China 3 State Power Investment Corporation Research Institute, Beijing 102209, China 4 Department of Nuclear Engineering and Radiological Sciences, University of Michigan, Ann Arbor, MI 48109, U.S.A.
Cite this article:
Ping DENG, Qunjia PENG, En-Hou HAN, Wei KE, Chen SUN, Haihong XIA, Zhijie JIAO. Study of Irradiation Damage in Domestically Fabricated Nuclear Grade Stainless Steel. Acta Metall Sin, 2017, 53(12): 1588-1602.
The radiation-induced segregation (RIS) and microstructure evolution such as dislocation loops and cavities are major microstructural causes for the irradiation-assisted stress corrosion cracking (IASCC) of austenitic stainless steel (SS) core components. While a couple of studies have been reported on the irradiation induced damage in nuclear grade (NG) austenitic SS, the evolution of dislocation loop density and size and its correlation with the mechanical properties have still remained incompletely understood. In addition, the correlation between the segregation at the grain boundary and that at the dislocation loop has received limited attentions. In particular, there is still a lack of a systematic study of the irradiation damage in domestically fabricated NG austenitic SS. In this work, the proton-irradiation induced microstructural damage in domestically fabricated 304NG SS was characterized, in an effort to correlate the RIS and the dislocation loop density and size with the irradiation dose, as well as the dislocation loop density and size with the radiation-induced hardening. The results revealed that the radiation-induced microstructure damage was mainly dislocation loops with a few micro-voids. The loop density was in the order of 1022 m-3 with an average size of <10 nm. The square root of the product of loop density and size (Nd)0.5, scaled linearly with the square root of irradiation dose with a factor of 6.8×103 dpa-0.5mm-1. The loops were believed to be mainly responsible for the hardening in 304NG SS, which also scaled linearly with (Nd)0.5 with a factor of 1.16×10-2 HV0.025mm. A comparative analysis about the segregation at the grain boundary and at the dislocation loop was conducted. While the depletion of Cr and enrichment of Ni at the dislocation loop and grain boundary showed no difference, the enrichment of Si at the dislocation loop could be of about 6 times of that at the grain boundary. In addition, the loop density and loop size, as well as RIS and radiation-induced hardening were all increased by a higher dose and tended to saturate by a dose of 3.0~5.0 dpa.
Fund: Supported by International Science & Technology Cooperation Program of China (No.2014DFA50800) and National Natural Science Foundation of China (No.51571204)
Fig.1 Schematic of irradiation specimen bars geometry (The irradiated region, hardness measurement positions and 3 mm TEM disks are highlighted by shaded area, red lines and circles, respectively)
Fig.2 Procedure for making 3DAP tips(a) the region of interest protected by Pt deposition(b) trenches cut around the Pt deposition(c) a microtip coupon with a couple of microtip posts(d) top view of the sample wedge sitting on the top of the post(e) Pt weld used to connect part of the sample wedge and the microtip post(f) the sample attached to the microtip post(g) side view of the sample post(h) view of the sample after cutting all round off(i) the final 3DAP tip
Fig.3 Bright-field TEM images of 304 stainless steel before (a) and after proton irradiation to a dose of 0.5 dpa (b), 1.5 dpa (c), 3.0 dpa (d) and 5.0 dpa (e) at 360 ℃, and the amplified image of a dislocation loop in Fig.3e (f)
Fig.4 Dark-field TEM images using g=200 (ZA [110]) showing dislocation components in 304 stainless steel before (a) and after proton irradiation to a dose of 0.5 dpa (b), 1.5 dpa (c), 3.0 dpa (d) and 5.0 dpa (e) at 360 ℃, and SAED pattern used for the dark-field TEM observation (f)
Fig.5 Loop size distributions in 304 stainless steel following proton irradiation at 360 ℃ to a dose of 0.5 dpa (a), 1.5 dpa (b), 3.0 dpa (c) and 5.0 dpa (d)
Fig.6 Measured changes in density and size of dislocation loops as a function of irradiation dose
Dose
N
d
Microhardness
Irradiation hardening
Δσ
dpa
1022 m-3
nm
HV0.025
HV0.025
MPa
0
-
-
190.9±12.6
-
-
0.5
0.364
5.81
247.8±11.8
56.9
160.4
1.5
1.423
7.25
294.2±20.7
103.3
354.3
3.0
1.804
8.61
332.3±17.8
141.4
434.7
5.0
2. 014
9.34
362.1±15.2
171.2
478.4
Table 1 Summary of microstructure and Vickers hardness measurements for 304 stainless steel following proton irradiation at 360 ℃
Fig.7 Bright field TEM images of voids in 304 stainless steel following proton irradiation at 360 ℃ to a dose of 0.5 dpa (a), 1.5 dpa (b), 3.0 dpa (c) and 5.0 dpa (d) (The voids are observed in slightly under-focused condition and highlighted by black arrows)
Fig.8 Radiation-induced segregation at the grain boundaries in 304 stainless steel
(a) bright field TEM image of a grain boundary in the unirradiated steel showing locations of EDS point- and line-scan analyses
(b~f) variations in the composition at grain boundaries in the steel following proton irradiation at 360 ℃ to a dose of unirradiated (b), 0.5 dpa (c), 1.5 dpa (d), 3.0 dpa (e) and 5.0 dpa (f)
(g) grain boundary composition variations with irradiation doses
Fig.9 3DAP atom maps showing radiation-induced segregation in 304 stainless steel following protons irradiation at 360 ℃ to a dose of 3.0 dpa (Enrichment of Si and depletion of Mn is evident. The dimension of the box is 69 nm×70 nm×220 nm)
Fig.10 3DAP atom isoconcentration surface plot of 304 stainless steel following irradiation to a dose of 3.0 dpa at 360 ℃
(a) dislocation loops and Si-rich clusters are more "visible" using Si isoconcentration surface plot at 2.5%
(b) overlap of isoconcentration surface plot of Si, Ni, Cr and Mn
(c) isoconcentration surface plot of Ni at 16% (green) and Si 2.5% (gray) showing enrichment of Ni at dislocation loops and Si-rich clusters
(d) isoconcentration surface plot of Cr at 12% (gold) and Si 2.5% (gray) showing depletion of Cr at dislocation loops and Si-rich clusters
(e) isoconcentration surface plot of Mn at 0.6% (blue) and Si 2.5% (gray) showing depletion of Mn at dislocation loops and Si-rich clusters
Fig.11 3DAP atom maps showing radiation-induced segregation at a dislocation loop highlighted by shaded area in Fig.10a in 304 stainless steel following irradiation to a dose of 3.0 dpa at 360 ℃ (a) and composition profile across the dislocation loop along the rectangle with dimensions of 4 nm×4 nm×40 nm in Fig.11a (b) (The arrows in Fig.11b show the approximate positions of the dislocation core)
Fig.12 Variations of microhardness as a function of irradiation dose (a) and variations of radiation-induced hardening (ΔH) as a function of the square root of irradiation dose (b)
Fig.13 Variations of the square root of the product of dislocation loop density and size (Nd)0.5 as a function of the square root of irradiation dose
Fig.14 Schematic showing vacancy and solute atom flows and composition changes for mechanisms of radiation-induced segregation
Fig.15 Radiation induced segregation at the grain boundary and at the dislocation loop in 304 stainless steel following irradiation to 3.0 dpa at 360 ℃ (a) and ratio of the segregation at dislocation loop to that at grain boundary (b)
Fig.16 Variations of irradiation-induced hardening (ΔH) as a function of the square root of the product of dislocation loop density and size
[1]
Stephenson K J, Was G S.Crack initiation behavior of neutron irradiated model and commercial stainless steels in high temperature water[J]. J. Nucl. Mater., 2014, 444: 331
[2]
Ioka I, Ishijima Y, Usami K, et al.Radiation hardening and IASCC susceptibility of extra high purity austenitic stainless steel[J]. J. Nucl. Mater., 2011, 417: 887
[3]
Fukuya K, Nakano M, Fujii K, et al.IASCC susceptibility and slow tensile properties of highly-irradiated 316 stainless steels[J]. J. Nucl. Sci. Technol., 2004, 41: 673
[4]
Ge?rard R, Somville F. Situation of the baffle-former bolts in Belgian units [A]. Proceeding 17th International Conference on Nuclear Engineering[C]. Brussels, Belgium: American Society of Mechanical Engineers, 2009: 521
[5]
Andersen P L, Ford F P, Murphy S M, et al.State of knowledge of radiation effects on environmental cracking in light water reactor core materials [A]. Proceeding 4th International Symposium on Environmental Degradation of Materials in Nuclear Power Systems-Water Reactors[C]. Houston: National Association of Corrosion Engineers, 1989: 83
[6]
Nishioka H, Fukuya K, Fujii K, et al.IASCC initiation in highly irradiated stainless steels under uniaxial constant load conditions[J]. J. Nucl. Sci. Technol., 2008, 45: 1072
[7]
Zhou R S, West E A, Jiao Z J, et al.Irradiation-assisted stress corrosion cracking of austenitic alloys in supercritical water[J]. J. Nucl. Mater., 2009, 395: 11
[8]
Was G S, Bruemmer S M.Effects of irradiation on intergranular stress corrosion cracking[J]. J. Nucl. Mater., 1994, 216: 326
[9]
Stephenson K J, Was G S.Comparison of the microstructure, deformation and crack initiation behavior of austenitic stainless steel irradiated in-reactor or with protons[J]. J. Nucl. Mater., 2015, 456: 85
[10]
Jiao Z J, Was G S, Miura T, et al.Aspects of ion irradiations to study localized deformation in austenitic stainless steels[J]. J. Nucl. Mater., 2014, 452: 328
[11]
Jiao Z, Was G S.Impact of localized deformation on IASCC in austenitic stainless steels[J]. J. Nucl. Mater., 2011, 408: 246
[12]
Jiao Z J, Was G S.Oxidation of a proton-irradiated 316 stainless steel in simulated BWR NWC environment [A]. Proceeding 15th International Conference on Environmental Degradation of Materials in Nuclear Power Systems-Water Reactors[C]. Chichster: John Wiley & Sons, 2011: 1329
[13]
Gan J, Was G S.Microstructure evolution in austenitic Fe-Cr-Ni alloys irradiated with rotons: Comparison with neutron-irradiated microstructures[J]. J. Nucl. Mater., 2001, 297: 161
[14]
Was G S.Recent developments in understanding irradiation assisted stress corrosion cracking [A]. Proceeding 11th International Conference on Environmental Degradation of Materials in Nuclear Power Systems-Water Reactors[C]. La Grange Park, IL: American Nuclear Society, 2003: 965
[15]
Bruemmer S M, Simonen E P, Scott P M, et al.Radiation-induced material changes and susceptibility to intergranular failure of light-water-reactor core internals[J]. J. Nucl. Mater., 1999, 274: 299
[16]
Edwards D J, Simonen E P, Bruemmer S M.Evolution of fine-scale defects in stainless steels neutron-irradiated at 275 ℃[J]. J. Nucl. Mater., 2003, 317: 13
[17]
Singh B N, Foreman A J E, Trinkaus H. Radiation hardening revisited: Role of intracascade clustering[J]. J. Nucl. Mater., 1997, 249: 103
[18]
Huang H F, Li J J, Liu R D, et al.Temperature effect of Xe ion irradiation to 316 austenitic stainless steel[J]. Acta Metall. Sin., 2014, 50: 1189(黄鹤飞, 李健健, 刘仁多等. 316奥氏体不锈钢离子辐照损伤中的温度效应研究[J]. 金属学报, 2014, 50: 1189)
[19]
Jiao Z, Was G S.The role of irradiated microstructure in the localized deformation of austenitic stainless steels[J]. J. Nucl. Mater., 2010, 407: 34
[20]
Gupta G, Jiao Z, Ham A N, et al.Microstructural evolution of proton irradiated T91[J]. J. Nucl. Mater., 2006, 351: 162
[21]
Gan J, Edwards D J, Simonen E P, et al.Microstructural evolution and hardening in 300-series stainless steels: Comparison between neutron and proton irradiations [A]. Proceeding 10th International Symposium on Environmental Degradation of Materials in Nuclear Power Systems-Water Reactors[C]. Houston: NACE International Publications, 2002 (in CD-ROM)
[22]
Jiao Z, Was G S.Novel features of radiation-induced segregation and radiation-induced precipitation in austenitic stainless steels[J]. Acta Mater., 2011, 59: 1220
[23]
Miller M K.Atom Probe Tomography: Analysis at the Atomic Level[M]. New York: Springer, 2012: 173
[24]
Liu W Q, Liu Q D, Gu J F.Development and application of atom probe tomography[J]. Acta Metall. Sin., 2013, 49: 1025(刘文庆, 刘庆冬, 顾剑锋. 原子探针层析技术(APT)最新进展及应用[J]. 金属学报, 2013, 49: 1025)
[25]
Sencer B H, Was G S, Sagisaka M, et al.Proton irradiation emulation of PWR neutron damage microstructures in solution annealed 304 and cold-worked 316 stainless steels[J]. J. Nucl. Mater., 2003, 323: 18
[26]
Wiedersich H, Okamoto P R, Lam N Q.A theory of radiation-induced segregation in concentrated alloys[J]. J. Nucl. Mater., 1979, 83: 98
[27]
Perks J M, Marwick A D, English C A.A Computer Code to Calculate Radiation-induced Segregation in Concentrated Ternary Alloys[M]. Harwell: AEA Technology, Atomic Energy Research Establishment, 1986: 48
[28]
Allen T R, Was G S.Modeling radiation-induced segregation in austenitic Fe-Cr-Ni alloys[J]. Acta Mater., 1998, 46: 3679
[29]
Rothman S J, Nowicki L J, Murch G E.Self-diffusion in austenitic Fe-Cr-Ni alloys[J]. J. Phys., 1980, 10F: 383
[30]
Allen T R, Was G S, Kenik E A.The effect of alloy composition on radiation-induced segregation in Fe-Cr-Ni alloys[J]. J. Nucl. Mater., 1997, 244: 278
[31]
Siegel R W. Vacancy concentrations in metals [J]. J. Nucl. Mater., 1978, 69-70: 117
[32]
Kiritani M, Takata H. Dynamic studies of defect mobility using high voltage electron microscopy [J]. J. Nucl. Mater., 1978, 69-70: 277
[33]
Allen T R, Busby J T, Was G S, et al.On the mechanism of radiation-induced segregation in austenitic Fe-Cr-Ni alloys[J]. J. Nucl. Mater., 1998, 255: 44
[34]
Lee E H, Maziasz P J, Rowcliffe A F, et al.Phase Stability during Irradiation[M]. Warrendale: TMS-AIME, 1981: 141
[35]
Was G S, Busby J T.Use of proton irradiation to determine IASCC mechanisms in light water reactors: Solute addition alloys [R]. Final Report, EPRI Project EP-P3038/C1434. Palo Alto, CA: Electric Power Research Institute, 2003 (in CD-ROM)
[36]
Wan Q M, Shu G G, Wang R S, et al.Study on the microstructure evolution of A508-3 steel under proton irradiarion[J]. Acta Metall. Sin., 2012, 48: 929(万强茂, 束国刚, 王荣山等. A508-3钢质子辐照条件下微结构演变研究[J]. 金属学报, 2012, 48: 929)
[37]
Li Z C, Chen L.Irradiation embrittlement mechanisms and relevant influence factors of nuclear reactor pressure vessel steels[J]. Acta Metall. Sin., 2014, 50: 1285(李正操, 陈良. 核能系统压力容器辐照脆化机制及其影响因素[J]. 金属学报, 2014, 50: 1285)
[38]
Li Z C, Abe H, Sekimura N.Detection of point defects upon ion irradiation by means of precipitate coherency[J]. J. Nucl. Mater., 2007, 362: 87
[39]
Higgy H R, Hammad F H.Effect of fast-neutron irradiation on mechanical properties of stainless steels: AISI types 304, 316 and 347[J]. J. Nucl. Mater., 1975, 55: 177
LIU Yi; LI Dingqiang; LIN Dongliang; CHEN Shipu(Shanghai Jiaotong University;200030;State Key Laboratory of Solid State Microstructures of Nanjing University; 210008);ZHAO Xiaoning;HONG Jianming(Nanjing University;210080)(Manuscript received 94-04-21). DISLOCATION FEATURES IN FeAl INTERMETALLIC COMPOUND AFTER DEFORMATION AT HIGH TEMPERATURE[J]. 金属学报, 1995, 31(1): 24-28.