Ti(C,N)薄膜的复合硬度与本征硬度的研究
徐可为;白辰东;何家文
西安交通大学金属材料强度国家重点实验室
ON THE COMPOSITE AND INTRINSIC HARDNESS OF Ti(C, N) FILMS
XU Kewei; BAI Chendong; HE Jiawen (State Key; Laboratory for Mechanical Behaviour of Materials; Hi'an Jiaotong University;Xi'an 710049)(Manuscript received 1994-08-23; in revised form 1995-01-26)
引用本文:

徐可为;白辰东;何家文. Ti(C,N)薄膜的复合硬度与本征硬度的研究[J]. 金属学报, 1995, 31(21): 429-434.
, , . ON THE COMPOSITE AND INTRINSIC HARDNESS OF Ti(C, N) FILMS[J]. Acta Metall Sin, 1995, 31(21): 429-434.

全文: PDF(429 KB)  
摘要: 本文对不同性质的膜─基体系通过确定C的具体取值对Joensson-Hogmark模型予以修正,研究厂等离子体增强化学气相沉积Ti(C,N)薄膜的硬度及其随成分组织的变化。Ti(C、N)薄膜具有较小的晶粒尺寸和较高的残余压应力,其硬度远高于一般的整体材料,在确定的。工艺条件下,其值上要取决于膜的含碳量,大体成线性增加关系。
关键词 : Ti(C,  N)薄膜,  复合硬皮,  本征硬度    
Abstract:The model proposed by Joensson and Hogmark takes the parameter, C, as a constant for different film-substrate systems. The parameter was modified in the present paper according to different hardness ratio of film to substrate and used them to study the variation of the hardness of PCVD Ti(C, N) films with the composition and the microstructure.Comparing with bulk materials, Ti(C, N) films have a relative high hardness due to the smaller crystal size and the higher compressive residual stress. It is controlled by the carbon content and hold a linear increase with the carbon content for a definite deposition technique.Correspondent:(XU Kewei, professor, Hi'an Jiaotong University, Hi'an 710049)
Key words: Ti(C    N) film    composite hardness    intrinsic hardness
    
基金资助:国家自然科学基金
1BueckleH.In:WestbrookJH,ConradH,eds.,ScienceofHardnessTestinganditsResearchApplications,MetalsPark,Ohio:ASM,1973.4532ValvodaV,CernyR,KuzelRJr.ThinSolidFilms,1988:158:2253DoernerMF,NixWD.JMaterRes.1986;1,6014WollenbergRL,PinchHL.In:ShielsSA,BagnallC,WitkowskiRE,VanderCFCoort.cds.,MicrostructuralScience,1987;13:175VingsboO,HogmarkS,JoenssonB,IngemarssonA.ASTMSTP889,1984:2576李恒德,肖纪美.材料的表面与界面,北京:清华大学出版社,19907TamuraM,KuboH.SurfCoatTechnol,1991;49:1948ThomasASurfaceEngineering,1987;3(2):1179PiviereJ,DelafondJ.SurfaceEngineering,1993;9(1):5910HedenqvistP,OlssonM,HogmarkS.SurfaceEngineering,1992;8(1):3911JoenssonB,HogmarksThinSolidFilms,1984;114:25712李世直,石玉龙,徐翔,赵程.薄膜科学与技术,1989;2(2):7013GeorgeUO.ExperimentalMechanics,1964;21(1):13514HuangRF,WenLS,GuoLPGongJ,YuBN,SurfCoatTechnol,1992;50:97(
[1] 吴铭方,刘飞,王凤江,乔岩欣. 陶瓷基复合材料辅助脉冲电流液相扩散连接的界面反应及接头强化机制[J]. 金属学报, 2015, 51(9): 1129-1135.
[2] 吴铭方, 匡泓锦, 王凤江, 林红香, 胥国祥. Zr/Cu/Zr部分瞬间液相焊扩散连接Ti(C, N)-Al2O3陶瓷基复合材料*[J]. 金属学报, 2014, 50(5): 619-625.
[3] 李新梅; 孙文磊; 憨勇; 刘炳 . 纯钛表面电解液微弧碳氮化制备碳氮化钛厚膜[J]. 金属学报, 2008, 44(9): 1105-1110 .
[4] 王全兆; 刘越; 关德慧; 于宝海; 陈志亮; 毕敬 . TiN含量对Ti(C, N)/NiCr金属陶瓷微观结构和力学性能的影响[J]. 金属学报, 2005, 41(11): 1121-1126 .
[5] 熊惟皓;胡镇华;崔崑. Ti(C,N)基金属陶瓷相界面层微晶结构的形成[J]. 金属学报, 1997, 33(5): 473-478.
[6] 熊惟皓;胡镇华;崔崑. Ti(C,N)基金属陶瓷的相界面过渡层[J]. 金属学报, 1996, 32(10): 1075-1080.
[7] 刘宁;赵兴中;江来珠;罗会国;胡镇华;崔崑. Ni粘结的Ti(C,N)金属陶瓷的横向断裂强度与断口的分形分析[J]. 金属学报, 1995, 31(5): 229-235.
[8] 刘长清;金柱京;吴维;戴少侠;李美栓;师昌绪. Ti(CN)涂层的宏观应力与破坏方式[J]. 金属学报, 1990, 26(1): 107-112.