不同服役条件下FGH96合金的蠕变特征
彭子超1(), 刘培元2, 王旭青1, 罗学军1, 刘健1, 邹金文1()
1.中国航发北京航空材料研究院 先进高温结构材料重点实验室 北京 100095
2.中国人民解放军陆军装备部航空军事代表局驻北京地区航空军事代表室 北京 100012
Creep Behavior of FGH96 Superalloy at Different Service Conditions
PENG Zichao1(), LIU Peiyuan2, WANG Xuqing1, LUO Xuejun1, LIU Jian1, ZOU Jinwen1()
1.Science and Technology on Advanced High Temperature Structural Materials Laboratory, AECC Beijing Institute of Aeronautical Materials, Beijing 100095, China
2.Aviation Military Representative Office of the PLA in Beijing, Beijing 100012, China
引用本文:

彭子超, 刘培元, 王旭青, 罗学军, 刘健, 邹金文. 不同服役条件下FGH96合金的蠕变特征[J]. 金属学报, 2022, 58(5): 673-682.
Zichao PENG, Peiyuan LIU, Xuqing WANG, Xuejun LUO, Jian LIU, Jinwen ZOU. Creep Behavior of FGH96 Superalloy at Different Service Conditions[J]. Acta Metall Sin, 2022, 58(5): 673-682.

全文: PDF(4862 KB)   HTML
摘要: 

采用SEM、EBSD和TEM等手段研究了FGH96合金在650~750℃、690~810 MPa条件下的蠕变特征,揭示FGH96合金在不同服役条件下的蠕变机理。结果表明,当蠕变温度为704℃时,FGH96合金的蠕变性能随着应力水平的提高而降低;当加载应力为690 MPa时,FGH96合金的蠕变性能随着温度提高而显著降低,且FGH96合金的稳态蠕变速率对服役温度更为敏感,服役温度每提高30℃,将会导致蠕变速率提高一个数量级。当温度处于650~750℃范围、应力处于690~810 MPa范围时,FGH96合金的蠕变变形均以位错滑移为主,且位错在滑移过程中,会在(111¯)原子面上形成大量的微孪晶。在不同服役条件下,FGH96合金的蠕变断裂均呈现典型的沿晶断裂特征。

关键词 : FGH96高温合金,  蠕变机理,  服役条件,  断裂特征    
Abstract:

The FGH96 superalloy is extensively used as a gas turbine disk under high temperature due to its excellent tensile and creep properties. With recent developments in the aviation industry, the velocity of the aircraft has increased significantly, thereby increasing the temperature and stress on the turbine disk materials during their service. Therefore, creep deformation is crucial in the turbine disk superalloy. In this study, the creep characteristics of FGH96 superalloy were systematically studied at 650-750oC and 690-810 MPa and the creep mechanism of the alloy under different service conditions was investigated via SEM, EBSD, and TEM. For the creep temperature of 704oC, the creep properties of the alloy decreased with the increase in stress level. When the applied loading stress was 690 MPa, the creep properties of FGH96 alloy decreased significantly with the increase in temperature, and its steady-state creep strain rate was more sensitive to the service temperature. Further, every 30oC increase in the service temperature increased the creep rate by an order of magnitude. For the temperature in the range 650-750oC and the applied loading stress in the range 690-810 MPa, the creep deformation of the alloy was dominated by dislocation slip and resulted in various micro-twins on the continuous (111¯) planes. Moreover, the creep fracture of FGH96 alloy presented typical intergranular fracture under different service conditions in this study.

Key words: FGH96 superalloy    creep mechanism    service condition    fracture feature
收稿日期: 2021-05-17     
ZTFLH:  TG132.32  
图1  蠕变试样及其解剖分析图
T / °Cσ / MPaεc
7046903% and fracture
720
750
780
810
6506901% and fracture
670
720
750
表1  FGH96合金蠕变实验方案
图2  1160℃固溶处理的FGH96合金试样的显微组织及γ'相尺寸分布
图3  FGH96合金蠕变曲线
图4  FGH96合金稳态蠕变速率随温度和应力的变化关系
T / oCσ / MPaγ˙ / s-1T / oCσ / MPaγ˙ / s-1
7046903.76 × 10-96506904.19 × 10-11
7207.82 × 10-96706.72 × 10-10
7501.76 × 10-87043.76 × 10-9
7802.74 × 10-87203.01 × 10-8
8104.98 × 10-87501.24 × 10-7
表2  不同条件下FGH96合金稳态蠕变速率
图5  704℃、不同加载应力条件下经过1.0%蠕变变形的FGH96合金局域取向差(KAM)和反极图(IPF)分析
图6  704℃、不同加载应力条件下经过1.0%蠕变变形的FGH96合金TEM像
图7  690 MPa应力、不同温度条件下经过1.0%蠕变变形的FGH96合金KAM和IPF分析
图8  FGH96合金在690 MPa、不同温度条件下蠕变后形成的微孪晶
图9  不同温度和应力条件下FGH96合金的蠕变断裂源区形貌
1 Zheng X L. Mechanical Properties of Materials [M]. 2nd Ed., Xi'an: Northwestern Polytechnical University Press, 1999: 114
1 郑修麟. 材料的力学性能 [M]. 第2版. 西安: 西北工业大学出版社, 1999: 114
2 Qu J S, Che X L, Song B. Effect of temperature and stress on creep behavior of welding joint in stainless steel [J]. Weld. Joining, 2003, (1): 17
2 屈金山, 车小莉, 宋 兵. 温度和应力对不锈钢焊接接头蠕变行为的影响 [J]. 焊接, 2003, (1): 17
3 Azadi M, Azadi M. Evaluation of high-temperature creep behavior in Inconel-713C nickel-based superalloy considering effects of stress levels [J]. Mater. Sci. Eng., 2017, A689: 298
4 Tian T, Hao Z B, Ge C C, et al. Effects of stress and temperature on creep behavior of a new third-generation powder metallurgy superalloy FGH100L [J]. Mater. Sci. Eng., 2020, A776: 139007
5 Hou Z P, Zhang S, Zhang P, et al. High temperature creep damage behavior of a novel Co-Cr-Mo-Ni alloy [J]. J. Iron Steel Res., 2019, 31: 683
5 侯智鹏, 张 姝, 张 鹏 等. 新型Cr-Co-Mo-Ni合金的高温蠕变损伤 [J]. 钢铁研究学报, 2019, 31: 683
6 Condat M, Decamps B. Shearing of γ' precipitates by single a/2<110> matrix dislocations in a γ/γ' Ni-based superalloy [J]. Scr. Metall., 1987, 21: 607
doi: 10.1016/0036-9748(87)90369-3
7 Décamps B, Morton A J, Condat M. On the mechanism of shear of γ' precipitates by single (a/2) <110> dissociated matrix dislocations in Ni-based superalloys [J]. Philos. Mag., 1991, 64A: 641
8 Décamps B, Raujol S, Coujou A, et al. On the shearing mechanism of γ' precipitates by a single (a/6)<112> Shockley partial in Ni-based superalloys [J]. Philos. Mag., 2004, 1A: 91
9 Knowles D M, Chen Q Z. Superlattice stacking fault formation and twinning during creep in γ/γ' single crystal superalloy CMSX-4 [J]. Mater. Sci. Eng., 2003, A340: 88
10 Chen Q Z, Knowles D M. Mechanism of <112> /3 slip initiation and anisotropy of γ' phase in CMSX-4 during creep at 750oC and 750 MPa [J]. Mater. Sci. Eng., 2003, A356: 352
11 Kolbe M. The high temperature decrease of the critical resolved shear stress in nickel-base superalloys [J]. Mater. Sci. Eng., 2001, A319-321: 383
12 Viswanathan G B, Sarosi P M, Whitis D H, et al. Deformation mechanisms at intermediate creep temperatures in the Ni-base superalloy René 88 DT [J]. Mater. Sci. Eng., 2005, A400-401: 489
13 Viswanathan G B, Karthikeyan S, Sarosi P M, et al. Microtwinning during intermediate temperature creep of polycrystalline Ni-based superalloys: Mechanisms and modelling [J]. Philos. Mag., 2006, 86A: 4823
14 Sarosi P M, Viswanathan G B, Mills M J. Direct observation of an extended complex stacking fault in the γ' phase of a Ni-base superalloy [J]. Scr. Mater., 2006, 55: 727
doi: 10.1016/j.scriptamat.2006.06.019
15 Unocic R R, Viswanathan G B, Sarosi P M, et al. Mechanisms of creep deformation in polycrystalline Ni-base disk superalloys [J]. Mater. Sci. Eng., 2008, A483-484: 25
16 Kovarik L, Unocic R R, Li J, et al. Microtwinning and other shearing mechanisms at intermediate temperatures in Ni-based superalloys [J]. Prog. Mater. Sci., 2009, 54: 839
doi: 10.1016/j.pmatsci.2009.03.010
17 Zou J W, Wang W X. Development and application of P/M superalloy [J]. J. Aeronaut. Mater., 2006, 26: 244
17 邹金文, 汪武祥. 粉末高温合金研究进展与应用 [J]. 航空材料学报, 2006, 26: 244
18 Zhang G Q, Zhang Y W, Zheng L, et al. Research progress in powder metallurgy superalloys and manufacturing technologies for aero-engine application [J]. Acta Metall. Sin., 2019, 55: 1133
18 张国庆, 张义文, 郑 亮 等. 航空发动机用粉末高温合金及制备技术研究进展 [J]. 金属学报, 2019, 55: 1133
19 Wang X Q, Luo X J, Zou J W. Effects of HIP temperature on microstructure of FGH96 superalloy [J]. J. Aeronaut. Mater., 2006, 26: 293
19 王旭青, 罗学军, 邹金文. 热等静压温度对FGH96粉末高温合金显微组织的影响 [J]. 航空材料学报, 2006, 26: 293
20 Peng Z C, Tian G F, Jiang J, et al. Mechanistic behaviour and modelling of creep in powder metallurgy FGH96 nickel superalloy [J]. Mater. Sci. Eng., 2016, A676: 441
21 Peng Z C, Zou J W, Wang X Q. Microstructural characterization of dislocation movement during creep in powder metallurgy FGH96 superalloy [J]. Mater. Today Commun., 2020, 25: 101361
22 Peng Z C, Zou J W, Yang J, et al. Influence of γ' precipitate on deformation and fracture during creep in PM nickel-based superalloy [J]. Prog. Nat. Sci., 2021, 31: 303
doi: 10.1016/j.pnsc.2020.12.008
23 Li M Z, Pham M S, Peng Z C, et al. Creep deformation mechanisms and CPFE modelling of a nickel-base superalloy [J]. Mater. Sci. Eng., 2018, A718: 147
24 Feng Y F, Zhou X M, Zou J W, et al. Effect of cooling rate during quenching on the microstructure and creep property of nickel-based superalloy FGH96 [J]. Int. J. Miner. Metall. Mater, 2019, 26: 493
25 Liu Q B, Lu C F, Yan P. Physicochemical phase analysis of a directionally solidified Ni-based cast superalloy [J]. Metall. Anal., 2006, 26(2): 9
25 刘庆斌, 卢翠芬, 燕 平. 一种定向凝固镍基铸造高温合金的物理化学相分析 [J]. 冶金分析, 2006, 26(2): 9
26 Kamaya M. Measurement of local plastic strain distribution of stainless steel by electron backscatter diffraction [J]. Mater. Charact., 2009, 60: 125
doi: 10.1016/j.matchar.2008.07.010
27 Kamaya M. A smoothing filter for misorientation mapping obtained by EBSD [J]. Mater. Trans., 2010, 51: 1516
doi: 10.2320/matertrans.MAW201005
28 Kamaya M. Assessment of local deformation using EBSD: Quantification of accuracy of measurement and definition of local gradient [J]. Ultramicroscopy, 2011, 111: 1189
doi: 10.1016/j.ultramic.2011.02.004
29 Kamaya M. Characterization of microstructural damage due to low-cycle fatigue by EBSD observation [J]. Mater. Charact., 2009, 60: 1454
doi: 10.1016/j.matchar.2009.07.003
[1] 谢君, 于金江, 孙晓峰, 金涛. K416B镍基铸造高温合金的700 ℃高周疲劳行为*[J]. 金属学报, 2016, 52(3): 257-263.
[2] 马宗义;吴胜进;罗明;吕毓雄;毕敬;张玉政. 弥散质点和SiC颗粒复合强化Al基复合材料 Ⅱ.性能和断裂特征[J]. 金属学报, 1994, 30(13): 33-38.