MICROSTRUCTURE OF RECRYSTALLIZATION AND THEIR EFFECTS ON STRESS RUPTURE PROPERTY OF SINGLE CRYSTAL SUPERALLOY DD6

  • Jichun XIONG ,
  • Jiarong LI ,
  • Fengli SUN ,
  • Shizhong LIU ,
  • Mei HAN
Expand
  • 1 Science and Technology on Advanced High Temperature Structural Materials Laboratory, Beijing Institute of Aeronautical Materials, Beijing 100095
    2 The 3rd Laboratory, Beijing Institute of Aeronautical Materials, Beijing 100095

Revised date: 2013-09-05

  Online published: 2014-06-20

Abstract

The specimens of single crystal superalloy DD6 were grit blasted and heat treated at 1100, 1200, and 1300 ℃ for 4 h at vacuum atmosphere respectively, then the microstructure of recrystallized DD6 alloy and their effects on the stress rupture performance were investigated. The results showed that cellular recrystallization nucleated in grit blasted samples heat treated at 1100 ℃ for 4 h, the dislocation tangles were found in the front of cellular recrystallization grain boundary in DD6 alloy, equiaxed recrystallization grains nucleated in grit blasted samples heat treated at 1300 ℃ for 4 h, and the carbides precipitate at the equiaxed recrystallization grain boundary, while the coexistence of equiaxed recrystallization grains and cellular recrystallization, defined as mixed recrystallization, occurred in the grit blasted samples heat treated at 1200 ℃ for 4 h. The cellular recrystallization reduced the stress rupture lives of DD6 alloy slightly, and the equiaxed recrystallization reduced stress rupture lives seriously, while the reduction degree of the stress rupture lives of the mixed recrystallization was between cellular recrystallization and equiaxed recrystallization. Besides this, with increase of depth of recrystallization and stress, the stresses rupture life decreased. It was also found that the fracture surface configuration was belonging to intergranular fracture with equiaxed recrystallization samples. The characteristic of the fracture surface changed to dimple fracture with cellular recrystallization samples, at all these condition the crack nucleated on the recrystallization grain boundaries of specimens during stress rupture process.

Cite this article

Jichun XIONG , Jiarong LI , Fengli SUN , Shizhong LIU , Mei HAN . MICROSTRUCTURE OF RECRYSTALLIZATION AND THEIR EFFECTS ON STRESS RUPTURE PROPERTY OF SINGLE CRYSTAL SUPERALLOY DD6[J]. Acta Metall Sin, 2014 , 50(6) : 737 -743 . DOI: 10.3724/SP.J.1037.2013.00561

References

[1] Gell M, Duhl D N, Giamei A F. In: Tien J K, Gell M, Maurer G, Wlodek S T eds., Superalloys 1980, Seven Springs, PA: TMS, 1980: 205
[2] Cetel A D, Duhl D N. In: Recichman S, Duhl D N, Maurer G, Antolovich S, Lund C eds., Superalloys 1988, Seven Springs, PA: TMS, 1988: 235
[3] Erickson G L. In: Kissinger R D, Deye D J, Anton D L, Cetel A D, Nathal M V, Pollock T M, Woodford D A eds., Superalloys 1996, Seven Springs, PA: TMS, 1996: 35
[4] Li J R, Zhong Z G, Tang D Z, Liu S Z, Wei P, Wei P Y, Wu Z T, Huang D, Han M. In: Pollock T M, Kissinger R D, Bowman R R, Green K A, McLean M, Olson S, Schirra J J eds., Superalloys 2000, Seven Springs, PA: TMS, 2000: 777
[5] Xiong J C, Li J R, Zhao J Q, Liu S Z. Acta Metall Sin, 2009; 45: 1232
[5] (熊继春, 李嘉荣, 赵金乾, 刘世忠. 金属学报, 2009; 45: 1232)
[6] Chen R Z. Aviat Eng Maint, 1990; 4: 22
[6] (陈荣章. 航空制造工程, 1990; 4: 22)
[7] Wei P, Li J R, Zhong Z Z. J Mater Eng, 2001; (10): 5
[7] (卫平, 李嘉荣, 钟振纲. 材料工程. 2001; (10): 5)
[8] Cox D C, Roebuck B, Rae C M F, Reed R C. Mater Sci Technol, 2003; 19: 440
[9] Li Y N, He D, Li S S, Han Y F. Acta Metall Sin, 2008; 44: 391
[9] (李亚楠, 何 迪, 李树索, 韩雅芳. 金属学报, 2008; 44: 391)
[10] Wang Z G, Zhao J C, Yan P, Zhou T T, Liu P Y. J Iron Steel Res, 2009; 21(2): 23
[10] (王志刚, 赵京晨, 燕 平, 周铁涛, 刘培英. 钢铁研究学报, 2009; 21(2): 23)
[11] Qu Y P, Liu L R, Zu G Q, Jin T, Hu Z Q. J Mater Eng, 2011; (8): 14
[11] (曲彦平, 刘丽荣, 祖国庆, 金涛, 胡壮麒. 材料工程, 2011; (8): 14)
[12] Bürgel R, Portella P D, Preuhs J. In: Pollock T M, Kissinger R D, Bowman R R, Green K A, McLean M, Olson S, Schirra J J eds., Superalloys 2000, Seven Springs, PA: TMS, 2000: 229
[13] Wang L, Xie G, Zhang J, Lou L H. Scr Mater, 2006; 55: 457
[14] Xie G, Zhang J, Lou L H. Scr Mater, 2008; 59: 858
[15] Xiong J C, Li J R, Liu S Z, Zhao J Q, Han M. Mater Charact, 2010; 61: 749
[16] Xie G, Wang L, Zhang J, Lou L H. Metall Mater Trans, 2008; 39A: 206
[17] Jo C Y, Cho H Y, Kim H M. Mater Sci Technol, 2003; 19: 1671
[18] Wang D L, Jin T, Yang S Q, Wei Z, Li J B, Hu Z Q. Mater Sci Forum, 2007; 546-549: 1229
[19] Xie G, Wang L, Zhang J, Lou L H. In: Reed R C, Green K A, Caron P, Gabb T P, Fahrmann M G, Huron E S, Woodard S A eds., Superalloy 2008, Seven Springs, PA: TMS, 2008: 453
[20] Li J R, Sun F L, Xiong J C, Liu S Z, Han M. Mater Sci Forum, 2010; 638-642: 2279
[21] Khan T, Caron P, Nakagawa Y G. J Met, 1986; 38(7): 16
[22] Zhang B, Liu D L, Tao C H, Jiang T. J Aero Mater, 2012; 32(6): 85
[22] (张兵, 刘德林, 陶春虎, 姜涛. 航空材料学报, 2012; 32(6): 85)
[23] Xiong J C, Li J R, Liu S Z, Han M. Chin J Nonferrous Met, 2010; 20: 1328
[23] (熊继春, 李嘉荣, 刘世忠, 韩梅. 中国有色金属学报, 2010; 20: 1328)
[24] Xiong J C, Li J R, Liu S Z. Chin J Aeronaut, 2010; 23: 478
[25] Li J R, Zhao J Q, Liu S Z, Han M. In: Reed R C, Green K A, Caron P, Gabb T P, Fahrmann M G, Huron E S, Woodard S A eds., Superalloys 2008, Seven Springs, PA: TMS, 2008: 443
[26] Zhang B, Lu X, Liu D L, Tao C H. Mater Sci Eng, 2012; A551: 149
[27] Meng J, Jin T, Sun X F, Hu Z Q. Mater Sci Eng, 2010; A527: 6119
Outlines

/