1 State Key Laboratory of Traction Power, Southwest Jiaotong University, Chengdu 610031, China 2 Shanghai Synchrotron Radiation Facility (SSRF), Shanghai Institute of Applied Physics, Chinese Academy of Sciences, Shanghai 201204, China
Cite this article:
Zhe SONG, Shengchuan WU, Yanan HU, Guozheng KANG, Yanan FU, Tiqiao XIAO. The Influence of Metallurgical Pores on Fatigue Behaviors of Fusion Welded AA7020 Joints. Acta Metall Sin, 2018, 54(8): 1131-1140.
With the rapid development of Chinese high-speed railway system, the urgent demand for lighter weight structures is increasing, and aluminum alloys are widely applied into manufacturing the railway train and critical safety components. As a medium strength aluminum alloy, the 7020 aluminum alloy shows a great potential. Hybrid laser welding has currently become one of the most important welding techniques for medium and high strength aluminum alloys. Nevertheless, intrinsic defects such as pores and shrinkages physically determine the fatigue resistance of the welded joint. Based on in situ synchrotron radiation X-ray computed microtomography (SR-μCT), the population, location and size of gas pores within AA7020 hybrid welded joints are firstly identified and counted. The critical size of gas pores, affecting the fatigue properties of welded joints, is acquired by combining the statistical results of the pores and the average grain size of the hybrid weld. Meanwhile, the qualitative relationship between pore size, effective stress and fatigue life is discussed through in situ fatigue life data via SR-μCT and fracture morphology. By using the finite element analysis, detailed works have been performed on the stress state near the pores of different positions inside the joint. Through the simulation analysis, the stress concentration coefficient around the pores firstly increases, then decreases, and finally tends to a stable trend as the location of the pore-like defect is transferred from the surface to the inside. Besides, the influence of porosity on fatigue crack initiation, fatigue crack growth and sudden breaking process is also analyzed using fatigue crack growth experiment. In conclusion, the results show that the critical pore size of hybrid laser welded joint can be qualitatively identified as 30 μm; the SR-μCT and fracture analysis show that larger surface and sub-surface pores are more likely to initiate fatigue cracks, and the fatigue crack propagation experiment further shows that the porosity has very little effect on the long crack growth but significant influence on the crack front.
Fund: Supported by National Natural Science Foundation of China (No.11572267), Science and Technology Research and Development Project of Sichuan Province (No.2017JY0216), Open Research Project of State Key Laboratory for Strength and Vibration of Mechanical Structures of Xi'an Jiaotong University (No.SV2016-KF-21)
Fig.1 Schematics of in-situ fatigue loading device based on synchrotron radiation X-ray tomography (a) principle diagram of operation (b) fatigue specimen size (unit: mm)
Fig.2 Statistical results of gas pores inside 10 in-situ imaging fatigue specimens at Shanghai synchrotron radiation facility (SSRF) and European synchrotron radiation facility (ESRF)
Fig.3 Position distribution of gas pores inside hybrid laser welded 7020 aluminum alloy from in situ imaging fatigue specimens at SSRF and ESRF
Fig.4 Synchrotron radiation X-ray based porosity imaging result of a typical 7020 aluminum alloy due to a hybrid laser welding process
Fig.5 Synchrotron radiation X-ray imaging result of process-induced pores inside a 7020 aluminum alloy due to a hybrid laser welding process
Fig.6 Schematics of the pore position classification in the welded joint (A—the square root of the projection area perpendicular to the load direction, h—the minimum distance between the boundary of the crack initiation pore and the free surface of the specimen) (a) h=0, as surface defect (b) h<A, as sub-surface defect (c) h>A, as internal defect
Specimen
Cracking source
A / μm
σmax / MPa
R
Nf / cyc
ESRF-1
Sub-surface pore
130.31
167
0.1
6700
SSRF-3
Surface pore
75.52
188
0.2
7400
SSRF-2
Sub-surface pore
67.71
214
0.2
22000
ESRF-3
Surface pore
121.26
173
0.1
24800
SSRF-5
Surface pore
80.67
217
0.2
26000
SSRF-1
Sub-surface pore
84.11
237
0.2
30000
ESRF-5
Sub-surface pore
78.43
137
0.1
40900
ESRF-4
Surface pore
109.60
148
0.1
47200
SSRF-4
Surface pore
132.77
144
0.2
77340
ESRF-2
Surface pore
57.81
143
0.1
88000
Table 1 Fatigue life data related with the defect location and affected area under in situ fatigue microtomography conducted at ESRF and SSRF
Fig.7 Specimen fracture morphologies at Nf =77340 cyc and crack initiation from a surface pore (a) macro morphology of fracture surface (b) fatigue source morphology (c) fatigue striation of stable propagation zone (d) final fracture region
Fig.8 S-N plot of the maximum effective stress (σeff) and Nf in fatigue test and synchrotron radiation X-ray in situ fatigue test
Fig.9 The relationship between the position of the pore and the upper surface of the weld in the simulation model and the boundary conditions of the finite element simulation (s—the distance from the pore center to the free surface (X-Y plane);r—the pore radius;S1—X-Z plane; L1—the intersection line of the X-Z plane and the bottom plane; U1, U2 and U3—the translational degrees of freedom along coordinate axis X direction, along coordinate axis Y direction, along coordinate axis Z direction, respectively, σ—the applied stress)
Fig.10 Principal stress fields across the pore parallel to X-Z plane (a) s/r =-0.2 (b) s/r =0 (c) s/r =2.7
Fig.11 Elastic and elastic-plastic simulations of stress concentration curves near the pores
Fig.12 Fatigue crack growth rates of three laser hybrid welded 7020 aluminum alloy joints under stress ratio R=0.1 and mean thickness t=1.84 mm
[1]
Yu C, Wu S C, Hu Y N, et al.Three-dimensional imaging of gas pores in fusion welded Al alloys by synchrotron radiation X-ray microtomography[J]. Acta Metall. Sin., 2015, 51: 159(喻程, 吴圣川, 胡雅楠等. 铝合金熔焊微气孔的三维同步辐射X射线成像[J]. 金属学报, 2015, 51: 159)
[2]
Zhang J, Lei Z, Wang X Y.Weld hot crack analysis of 6005A aluminum alloy profile for high-speed train[J]. Trans. China Weld. Inst., 2012, 33(8): 60(张健, 雷振, 王旭友. 高速列车6005A铝合金型材焊接热裂纹分析[J]. 焊接学报, 2012, 33(8): 60)
[3]
Wu S C, Zhu Z T, Li X W.Laser Welding of Aluminum Alloys and the Performance Evaluation [M]. Beijing: National Defense Industry Press, 2014: 18(吴圣川, 朱宗涛, 李向伟. 铝合金的激光焊接及性能评价 [M]. 北京: 国防工业出版社, 2014: 18)
[4]
Vanderesse N, Maire é, Chabod A, et al.Microtomographic study and finite element analysis of the porosity harmfulness in a cast aluminium alloy[J]. Int. J. Fatigue, 2011, 33: 1514
[5]
Buffière J Y, Savelli S, Jouneau P H, et al.Experimental study of porosity and its relation to fatigue mechanisms of model Al-Si7-Mg0.3 cast Al alloys[J]. Mater. Sci. Eng., 2001, A316: 115
[6]
Wang Q G, Apelian D, Lados D A.Fatigue behavior of A356-T6 aluminum cast alloys. Part I. Effect of casting defects[J]. J. Light Met., 2001, 1: 73
[7]
Zhang B, Chen W, Poirier D R.Effect of solidification cooling rate on the fatigue life of A356.2-T6 cast aluminium alloy[J]. Fatigue Fract. Eng. Mater. Struct., 2000, 23: 417
[8]
Toda H, Masuda S, Batres R, et al.Statistical assessment of fatigue crack initiation from sub-surface hydrogen micropores in high-quality die-cast aluminum[J]. Acta Mater., 2011, 59: 4990
[9]
Wu S C, Xiao T Q, Withers P J.The imaging of failure in structural materials by synchrotron radiation X-ray microtomography[J]. Eng. Fract. Mech., 2017, 182: 127
[10]
Brochu M, Verreman Y, Ajersch F, et al.High cycle fatigue strength of permanent mold and rheocast aluminum 357 alloy[J]. Int. J. Fatigue, 2010, 32: 1233
[11]
Serrano-Munoz I, Buffiere J Y, Mokso R, et al.Location, location & size: Defects close to surfaces dominate fatigue crack initiation[J]. Sci. Rep., 2017, 7: 45239
[12]
Serrano-Munoz I, Buffiere J Y, Verdu C, et al.Influence of surface and internal casting defects on the fatigue behaviour of A357-T6 cast aluminium alloy[J]. Int. J. Fatigue, 2016, 82: 361
[13]
Mu P, Nadot Y, Nadot-Martin C, et al.Influence of casting defects on the fatigue behavior of cast aluminum AS7G06-T6[J]. Int. J. Fatigue, 2014, 63: 97
[14]
Wu S C, Hu Y N, Fu Y N, et al.Study on fatigue cracking of welded aluminum alloys via in situ synchrotron radiation X-ray microtomography[J]. Trans. China Weld. Inst., 2015, 36(12): 5(吴圣川, 胡雅楠, 付亚楠等. 铝合金焊缝疲劳开裂的原位同步辐射X射线成像[J]. 焊接学报, 2015, 36(12): 5)
[15]
Wu S C, Yu C, Yu P S, et al.Corner fatigue cracking behavior of hybrid laser AA7020 welds by synchrotron X-ray computed microtomography[J]. Mater. Sci. Eng., 2016, A651: 604
[16]
Wu S C, Yu C, Zhang W H, et al.Porosity induced fatigue damage of laser welded 7075-T6 joints investigated via synchrotron X-ray microtomography[J]. Sci. Technol. Weld. Join., 2015, 20: 11
[17]
Yadollahi A, Shamsaei N.Additive manufacturing of fatigue resistant materials: Challenges and opportunities[J]. Int. J. Fatigue, 2017, 98: 14
[18]
Hu Y N, Wu S C, Zhang S Q, et al.Three-dimensional X-ray micro-tomography based microstructure and mechanical performance of hybrid laser welded AA7020[J]. Chin. J. Lasers, 2016, 43: 84(胡雅楠, 吴圣川, 张思齐等. 基于三维X射线成像的激光复合焊接7020铝合金的组织与力学特性演变[J]. 中国激光, 2016, 43: 84)
[19]
Ferrié E, Buffière J Y, Ludwig W.3D characterisation of the nucleation of a short fatigue crack at a pore in a cast Al alloy using high resolution synchrotron microtomography[J]. Int. J. Fatigue, 2005, 27: 1215
[20]
Murakami Y.Metal Fatigue: Effects of Small Defects and Nonmetallic Inclusions[M]. Oxford: Elsevier, 2002: 44
[21]
Xu Z Q, Wen W, Zhai T G.Effects of pore position in depth on stress/strain concentration and fatigue crack initiation[J]. Metall. Mater. Trans., 2012, 43A: 2763
[22]
Tammas-Williams S, Withers P J, Todd I, et al.The influence of porosity on fatigue crack initiation in additively manufactured titanium components[J]. Sci. Rep., 2017, 7: 7308
[23]
Li P, Lee P D, Maijer D M, et al.Quantification of the interaction within defect populations on fatigue behavior in an aluminum alloy[J]. Acta Mater., 2009, 57: 3539
[24]
Walker K.The effect of stress ratio during crack propagation and fatigue for 2024-T3 and 7075-T6 aluminum [A]. Effects of Environment and Complex Load History on Fatigue Life[C]. West Conshohocken, PA: ASTM, 1970, 462: 1
[25]
Dowling N E, Calhoun C A, Arcari A.Mean stress effects in stress-life fatigue and the Walker equation[J]. Fatigue Fract. Eng. Mater. Struct., 2009, 32: 163
[26]
Borbély A, Mughrabi H, Eisenmeier G, et al.A finite element modelling study of strain localization in the vicinity of near-surface cavities as a cause of subsurface fatigue crack initiation[J]. Int. J. Fract., 2002, 115: 227
[27]
Dezecot S, Maurel V, Buffiere J Y, et al.3D characterization and modeling of low cycle fatigue damage mechanisms at high temperature in a cast aluminum alloy[J]. Acta Mater., 2017, 123: 24
[28]
Gerard D A, Koss D A.The influence of porosity on short fatigue crack growth at large strain amplitudes[J]. Int. J. Fatigue, 1991, 13: 345
[29]
Mo D F, He G Q, Hu Z F, et al.Effect of porosity on fatigue property in aluminum cast alloys[J]. J. Mater. Eng., 2010, (7): 92(莫德锋, 何国求, 胡正飞等. 孔洞对铸造铝合金疲劳性能的影响[J]. 材料工程, 2010, (7): 92)
[30]
Paris P C, Erdogan F.A critical analysis of crack propagation laws[J]. J. Basic Eng., 1963, 85: 528
[31]
Zhang H, Toda H, Hara H, et al.Three-dimensional visualization of the interaction between fatigue crack and micropores in an aluminum alloy using synchrotron X-ray microtomography[J]. Metall. Mater. Trans., 2007, 38A: 1774
[32]
Tsay L W, Shan Y P, Chao Y H, et al.The influence of porosity on the fatigue crack growth behavior of Ti-6Al-4V laser welds[J]. J. Mater. Sci., 2006, 41: 7498