添加Ti对Fe22Cr5Al3Mo合金在500℃过热蒸汽中腐蚀行为的影响
收稿日期: 2021-05-12
修回日期: 2021-09-05
网络出版日期: 2021-09-22
基金资助
国家自然科学基金项目(51871141)
Effect of Ti on the Corrosion Behavior of Fe22Cr5Al3Mo Alloy in 500oC Superheated Steam
Received date: 2021-05-12
Revised date: 2021-09-05
Online published: 2021-09-22
Supported by
National Natural Science Foundation of China(51871141)
利用真空非自耗电弧炉熔炼了3种Fe22Cr5Al3Mo-xTi (x = 0、0.5、1.0,质量分数,%)合金,在静态高压釜中进行500℃、10.3 MPa过热蒸汽的腐蚀实验。采用XRD、OM、FIB/SEM、EDS和TEM观察分析腐蚀前后样品的显微组织、晶体结构和成分。结果表明,3种合金腐蚀不同时间形成的氧化膜均发生了分层现象,氧化膜外层均为Fe2O3,中间层均为hcp-Cr2O3,内层均为Al2O3;在靠近氧化膜和合金界面处的Al2O3膜中存在α-(Fe, Cr)。0Ti、0.5Ti和1.0Ti合金的Cr氧化膜厚度与氧化膜总厚度的比值(R)遵循R0.5Ti > R1.0Ti > R0Ti,这说明与0Ti和1.0Ti相比0.5Ti合金的耐腐蚀性能最优。添加Ti可抑制合金中Cr23C6第二相的析出,降低合金的氧化膜总厚度,提高保护性hcp-Cr2O3膜的厚度,从而提高合金的耐腐蚀性能。
孙蓉蓉 , 姚美意 , 林晓冬 , 张文怀 , 仇云龙 , 胡丽娟 , 谢耀平 , 杨健 , 董建新 , 成国光 . 添加Ti对Fe22Cr5Al3Mo合金在500℃过热蒸汽中腐蚀行为的影响[J]. 金属学报, 2022 , 58(5) : 610 -622 . DOI: 10.11900/0412.1961.2021.00200
Zirconium alloys can react with water to produce hydrogen under a loss of coolant accident, which can lead to a hydrogen explosion. Therefore, the idea of developing accident tolerant fuel (ATF) is proposed, which involves nuclear fuel and cladding. FeCrAl alloy is a promising candidate material for ATF cladding. Studying the effects of alloying elements on the corrosion behavior and mechanism of FeCrAl alloy can provide a theoretical basis and guidance for optimizing its composition. Therefore, in this study, the effect of Ti on the corrosion behavior of Fe22Cr5Al3Mo alloy in 500oC superheated steam was investigated. Three types of Fe22Cr5Al3Mo-xTi (x = 0, 0.5, 1.0, mass fraction, %) alloys, designated as 0Ti, 0.5Ti, and 1.0Ti alloys, respectively, were fabricated and corroded in 500oC and 10.3 MPa superheated steam using a static autoclave. The microstructure, crystal structure and composition of the samples before and after corrosion were observed using XRD, OM, FIB/SEM, EDS, and TEM. The results show that the oxide films formed on the Fe22Cr5Al3Mo-xTi alloys in 500oC and 10.3 MPa superheated steam present a trilayer structure consisting of an outer oxide layer of Fe2O3, a middle layer of hcp-Cr2O3, and an inner layer of Al2O3. There is α-(Fe, Cr) in the Al2O3 layer near the oxide/metal interface. The ratio, R, of Cr oxide film thickness to total oxide film thickness for 0Ti, 0.5Ti, and 1.0Ti alloys follows the order R0.5Ti > R1.0Ti > R0Ti, which may explain the better corrosion resistance of 0.5Ti alloy than 1.0Ti and 0Ti alloys. The addition of Ti can reduce the total thickness of the oxide films and improve the corrosion resistance of the alloys by increasing the thickness of the protective hcp-Cr2O3 film and inhibiting the precipitation of Cr23C6.
Key words: FeCrAl alloy; Ti; corrosion; oxide film; microstructure
| 1 | Zinkle S J, Terrani K A, Gehin J C, et al. Accident tolerant fuels for LWRs: A perspective [J]. J. Nucl. Mater., 2014, 448: 374 |
| 2 | Little E A, Stow D A. Void-swelling in irons and ferritic steels: II. An experimental survey of materials irradiated in a fast reactor [J]. J. Nucl. Mater., 1979, 87: 25 |
| 3 | Lim J, Hwang I S, Kim J H. Design of alumina forming FeCrAl steels for lead or lead-bismuth cooled fast reactors [J]. J. Nucl. Mater., 2013, 441: 650 |
| 4 | Pint B A, Terrani K A, Yamamoto Y, et al. Material selection for accident tolerant fuel cladding [J]. Metall. Mater. Trans., 2015, 2: 190 |
| 5 | Lim J, Nam H O, Hwang I S, et al. A study of early corrosion behaviors of FeCrAl alloys in liquid lead-bismuth eutectic environments [J]. J. Nucl. Mater., 2010, 407: 205 |
| 6 | Engkvist J, Bexell U, Grehk M, et al. High temperature oxidation of FeCrAl-alloys-influence of Al-concentration on oxide layer characteristics [J]. Mater. Corros., 2009, 60: 876 |
| 7 | Pint B A, Unocic K A, Terrani K A. Effect of steam on high temperature oxidation behaviour of alumina-forming alloys [J]. Mater. High Temp., 2015, 32: 28 |
| 8 | Kögler R, Anwand W, Richter A, et al. Nanocavity formation and hardness increase by dual ion beam irradiation of oxide dispersion strengthened FeCrAl alloy [J]. J. Nucl. Mater., 2012, 427: 133 |
| 9 | Sun Z Q, Bei H B, Yamamoto Y. Microstructural control of FeCrAl alloys using Mo and Nb additions [J]. Mater. Charact., 2017, 132: 126 |
| 10 | Dolley E J, Schuster M, Crawford C, et al. Mechanical behavior of FeCrAl and other alloys following exposure to LOCA conditions plus quenching [A]. Proceedings of the 18th International Conference on Environmental Degradation of Materials in Nuclear Power Systems-Water Reactors [C]. Switzerland: Springer International Publishing, 2018: 185 |
| 11 | Park D J, Kim H G, Park J Y, et al. A study of the oxidation of FeCrAl alloy in pressurized water and high-temperature steam environment [J]. Corros. Sci., 2015, 94: 459 |
| 12 | Badini C, Laurella F. Oxidation of FeCrAl alloy: Influence of temperature and atmosphere on scale growth rate and mechanism [J]. Surf. Coat. Technol., 2001, 135: 291 |
| 13 | Rebak R B. Versatile oxide films protect FeCrAl alloys under normal operation and accident conditions in light water power reactors [J]. JOM, 2018, 70: 176 |
| 14 | Chu R. Studies on high-temperature oxidation and its influence mechanism of Fe-Cr-Al alloy [D]. Shenyang: Shenyang Normal University, 2013 |
| 14 | 褚 冉. Fe-Cr-Al合金高温氧化及影响机理研究 [D]. 沈阳: 沈阳师范大学, 2013 |
| 15 | Herbelin J M, Mantel M, Cogne J Y. Future trends of FeCrAl alloys for automative catalytic converters to reach mass production [Z]. Germany: Werkstoff-Informationsgesellschaft mbH, Frankfurt am Main, 1997: 79 |
| 16 | Ning F Q, Wang X, Yang Y, et al. Uniform corrosion behavior of FeCrAl alloys in borated and lithiated high temperature water [J]. J. Mater. Sci. Technol., 2021, 70: 136 |
| 17 | Kitajima Y, Hayashi S, Ukai S, et al. The effect of additional elements on oxide scale evolution of Fe-20at.%Cr-10at.%Al alloy at 900℃ in air [J]. Mater. Sci. Forum., 2008, 595-598: 1013 |
| 18 | Huang T H, Naumenko D, Song P, et al. Effect of titanium addition on alumina growth mechanism on yttria-containing FeCrAl-base alloy [J]. Oxid. Met., 2018, 90: 671 |
| 19 | Schutze M. Lifetime Modelling of High Temperature Corrosion Processes EFC 34 [M]. Boca Raton, FL, USA: CRC Press, 2001: 66 |
| 20 | Dang J, Zhou P, Shi H Y. Influence of Nb/Ti on corrosion resistance properties of low chromium ferritic stainless steels [J]. Iron Steel Van Tit, 2020, 41: 147 |
| 20 | 党 杰, 周 鹏, 史洪源. Nb、Ti对低铬铁素体不锈钢腐蚀性能的影响 [J]. 钢铁钒钛, 2020, 41: 147 |
| 21 | Li X, Lu X L, Bi H Y. Effect of Nb, Ti on the properties of 15Cr ferritic stainless steel [A]. Proceedings of the 8th (2011) China Iron and Steel Annual Meeting [C]. Beijing: Metallurgical Industry Press, 2011: 535 |
| 21 | 李 鑫, 陆晓莉, 毕洪运. Nb、Ti对15Cr铁素体不锈钢性能的影响 [A]. 第八届(2011)中国钢铁年会论文集 [C]. 北京: 冶金工业出版社, 2011: 535 |
| 22 | Zhang X, Sun Q S, Du W. Effect of Nb, Ti on structure and property of ultra-low carbon and nitrogen ferritic stainless steel [A]. Proceedings of the 4th Annual Youth Academic Conference of China Society of Metals [C]. Beijing: Iron & Steel, 2008: 138 |
| 22 | 张 鑫, 孙全社, 杜 伟. Nb、Ti对超低碳氮430铁素体不锈钢组织和性能的影响 [A]. 第4届中国金属学会青年学术年会论文集 [C]. 北京: 钢铁, 2008: 138 |
| 23 | Yu Y N. Fundamentals of Materials Science [M]. Beijing: Higher Education Press, 2006: 781 |
| 23 | 余永宁. 材料科学基础 [M]. 北京: 高等教育出版社, 2006: 781 |
| 24 | Qian Y, Sun R R, Zhang W H, et al. Effect of Nb on microstructure and corrosion resistance of Fe22Cr5Al3Mo alloy [J]. Acta Metall. Sin., 2020, 56: 321 |
| 24 | 钱 月, 孙蓉蓉, 张文怀 等. Nb对Fe22Cr5Al3Mo合金显微组织和耐腐蚀性能的影响 [J]. 金属学报, 2020, 56: 321 |
| 25 | Li N, Parker S S, Wood E S, et al. Oxide morphology of a FeCrAl alloy, Kanthal APMT, following extended aging in air at 300oC to 600oC [J]. Metall. Mater. Trans., 2018, 49A: 2940 |
| 26 | Li N, Parker S S, Saleh T A, et al. Intermediate temperature corrosion behaviour of Fe-12Cr-6Al-2Mo-0.2Si-0.03Y alloy (C26M) at 300-600oC [J]. Corros. Sci., 2019, 157: 274 |
| 27 | Dai J X, Gong Z M, Xu S T, et al. In situ study on the initial oxidation behavior of zirconium alloys with near-ambient pressure XPS [J]. Acta Phys. Chim. Sin., 2020, 36: 2003026 |
| 27 | 戴久翔, 龚忠苗, 徐诗彤 等. 锆合金初始氧化行为的原位近常压XPS研究 [J]. 物理化学学报, 2020, 36: 2003026 |
| 28 | Pan D, Zhang R Q, Wang H J, et al. In steam short-time oxidation kinetics of FeCrAl alloys [J]. J. Mater. Eng. Perform., 2018, 27: 6407 |
| 29 | Zhang Z G, Niu Y, Zhang X J. Effect of third element Cr in Fe-Cr-Al alloys [J]. J. Iron Steel Res., 2007, 19: 46 |
| 29 | 张志刚, 牛 焱, 张学军. 铁-铬-铝合金中铬的第三组元作用 [J]. 钢铁研究学报, 2007, 19: 46 |
| 30 | Terrani K A, Pint B A, Kim Y J, et al. Uniform corrosion of FeCrAl alloys in LWR coolant environments [J]. J. Nucl. Mater., 2016, 479: 36 |
| 31 | Pint B A, Terrani K A, Rebak R B. Steam oxidation behavior of FeCrAl cladding [A]. Proceedings of the 18th International Conference on Environmental Degradation of Materials in Nuclear Power Systems-Water Reactors [C]. Switzerland: Springer International Publishing, 2018: 235 |
/
| 〈 |
|
〉 |