模压变形中国低活化马氏体钢沉淀相对其力学性能的影响
收稿日期: 2020-08-26
修回日期: 2020-10-20
网络出版日期: 2020-12-21
基金资助
国家自然科学基金项目(51875158)
Influence of Precipitation of China Low Activation Martensitic Steel on Its Mechanical Properties After Groove Pressing
Received date: 2020-08-26
Revised date: 2020-10-20
Online published: 2020-12-21
Supported by
National Natural Science Foundation of China(51875158)
采用室温拉伸、500℃高温拉伸、显微硬度、SEM、TEM等方法研究中国低活化马氏体钢(CLAM钢)多道次模压变形诱导沉淀相回溶和析出对力学性能的影响。结果表明,三道次模压变形后,有效细化了晶粒和沉淀相,尺寸为5 μm以上的晶粒所占体积分数减小为0.49%,M23C6相和MX相平均尺寸分别从107.32和17.12 nm减小到93.97和13.59 nm。累积应变为2.32时,抗拉强度和硬度分别为720 MPa和2.46 GPa,较变形前分别增加了22.87%和12.33%;当累积应变达到3.48时,与累积应变为2.32时相比其强度降低了4.31%,硬度和延伸率分别上升了2.03%和6.27%,该变化与变形过程中发生明显的沉淀相回溶有关。
薛克敏 , 盛杰 , 严思梁 , 田文春 , 李萍 . 模压变形中国低活化马氏体钢沉淀相对其力学性能的影响[J]. 金属学报, 2021 , 57(7) : 903 -912 . DOI: 10.11900/0412.1961.2020.00329
In this work, a constrained groove pressing experiment was carried out to investigate the influence of constrained groove pressing on precipitated phase dissolution and mechanical properties of China low activation martensitic (CLAM) steels. The aim of this study is to improve the comprehensive service performances of CLAM steels used in the first wall of fusion reactor cladding. The influence of the dissolution and precipitation of precipitates on the mechanical properties of CLAM steel subjected to multi-pass groove pressing was investigated via tensile tests at room temperature and 500oC, microhardness tests, SEM, and TEM. The results show that the grains and precipitated phases are effectively refined after three passes of groove pressing, the volume fraction of grains above 5 μm is reduced to 0.49%, and the average size of M23C6 and MX phases is reduced from 107.32 and 17.12 nm to 93.97 and 13.59 nm, respectively. When the cumulative strain of the billets reaches a value of 2.32 (pass two), the tensile strength and microhardness are found to be 720 MPa and 2.46 GPa, respectively. When the cumulative strain increases to 3.48 (pass three), the strength of the CLAM steel decreases by 4.31%, whereas the microhardness and elongation increase by 2.03% and 6.27%, respectively. These trends are related to the evident dissolution of the precipitates during the deformation process.
| 1 | Tan W X. Effect of heat treatment on microstructure and mechanical properties of low activation ferrite/martensitic steels used for the fusion reactor [D]. Wuhan: Huazhong University of Science and Technology, 2011 |
| 1 | 谭文霞. 聚变堆用低活化钢的热处理改性及微观组织和性能研究 [D]. 武汉: 华中科技大学, 2011 |
| 2 | Xu Y P, Lyu Y M, Zhou H S, et al. A review on the development of the structural materials of the fusion blanket [J]. Mater. Rev., 2018, 32: 2897 |
| 2 | 徐玉平, 吕一鸣, 周海山等. 核聚变堆包层结构材料研究进展及展望 [J]. 材料导报, 2018, 32: 2897 |
| 3 | Tan L, Hoelzer D T, Busby J T, et al. Microstructure control for high strength 9Cr ferritic-martensitic steels [J]. J. Nucl. Mater., 2012, 422: 45 |
| 4 | van der Schaaf B, Tavassoli F, Fazio C, et al. The development of EUROFER reduced activation steel [J]. Fusion Eng. Des., 2003, 69: 197 |
| 5 | Klueh R L, Gelles D S, Jitsukawa S, et al. Ferritic/martensitic steels—Overview of recent results [J]. J. Nucl. Mater., 2002, 307-311: 455 |
| 6 | Shankar V, Mariappan K, Sandhya R, et al. Long term creep-fatigue interaction studies on India-specific reduced activation ferritic-martensitic (IN-RAFM) steel [J]. Int. J. Fatigue, 2017, 98: 259 |
| 7 | Yuan D Q, Ma H L, Fan P, et al. Synergistic effect on formation of radiation damage in CLAM steel studied by triple beam irradiation [J]. Defect Diffus. Forum, 2017, 373: 117 |
| 8 | Taneike M, Sawada K, Abe F. Effect of carbon concentration on precipitation behavior of M23C6 carbides and MX carbonitrides in martensitic 9Cr steel during heat treatment [J]. Metall. Mater. Trans., 2004, 35A: 1255 |
| 9 | Wang H, Yan W, van Zwaag S, et al. On the 650oC thermostability of 9-12Cr heat resistant steels containing different precipitates [J]. Acta Mater., 2017, 134: 143 |
| 10 | Liu S J, Huang Q Y, Peng L, et al. Microstructure and its influence on mechanical properties of CLAM steel [J]. Fusion Eng. Des., 2012, 87: 1628 |
| 11 | Zhong B Y, Huang B, Li C J, et al. Creep deformation and rupture behavior of CLAM steel at 823 K and 873 K [J]. J. Nucl. Mater., 2014, 455: 640 |
| 12 | Li M S, Yang S. Effect of heat treatment on the microstructure and properties of 9Cr2WVTa reduced activation steels [A]. Energy Materials Conference Proceedings 2014 [C]. Oxford, England: Blackwell Science Publ., 2014: 551 |
| 13 | Aydogan E, Chen T, Gigax J G, et al. Effect of self-ion irradiation on the microstructural changes of alloy EK-181 in annealed and severely deformed conditions [J]. J. Nucl. Mater., 2017, 487: 96 |
| 14 | Lee S H, Saito Y, Tsuji N, et al. Role of shear strain in ultragrain refinement by accumulative roll-bonding (ARB) process [J]. Scr. Mater., 2002, 46: 281 |
| 15 | Huang J Y, Zhu Y T, Alexander D J, et al. Development of repetitive corrugation and straightening [J]. Mater. Sci. Eng., 2004, A371: 35 |
| 16 | Yang K H, Peng K P, Chen W Z. Microstructural evolution and grain refinement of 1060 pure Al processed by constrained groove pressing [J]. Chin. J. Nonferrous Met., 2011, 21: 3026 |
| 16 | 杨开怀, 彭开萍, 陈文哲. 限制模压变形1060纯铝的组织演化与晶粒细化 [J]. 中国有色金属学报, 2011, 21: 3026 |
| 17 | Shin D H, Park J J, Kim Y S, et al. Constrained groove pressing and its application to grain refinement of aluminum [J]. Mater. Sci. Eng., 2002, A328: 98 |
| 18 | Wang Z S. Experimental and numerical study on constrained groove pressing of sheet metals [D]. Jinan: Shandong University, 2014 |
| 18 | 王宗申. 金属板材限制模压变形工艺的实验与数值模拟研究 [D]. 济南: 山东大学, 2014 |
| 19 | Ukai S, Mizuta S, Fujiwara M, et al. Development of 9Cr-ODS martensitic steel claddings for fuel pins by means of ferrite to austenite phase transformation [J]. J. Nucl. Sci. Technol., 2002, 39: 778 |
| 20 | Wang D, Zhang J, Lou L H. Formation and stability of nano-scaled M23C6 carbide in a directionally solidified Ni-base superalloy [J]. Mater. Charact., 2009, 60: 1517 |
| 21 | Shtansky D V, Nakai K, Ohmori Y. Crystallography and structural evolution during reverse transformation in an Fe-17Cr-0.5C tempered martensite [J]. Acta Mater., 2000, 48: 1679 |
| 22 | Armaki H G, Chen R P, Maruyama K, et al. Creep behavior and degradation of subgrain structures pinned by nanoscale precipitates in strength-enhanced 5 to 12 pct Cr ferritic steels [J]. Metall. Mater. Trans, 2011, 42A: 3084 |
| 23 | Dudova N, Plotnikova A, Molodov D, et al. Structural changes of tempered martensitic 9%Cr-2%W-3%Co steel during creep at 650°C [J]. Mater. Sci. Eng., 2012, A534: 632 |
| 24 | Xiao X, Liu G Q, Hu B F, et al. Coarsening behavior for M23C6 carbide in 12%Cr-reduced activation ferrite/martensite steel: Experimental study combined with DICTRA simulation [J]. J. Mater. Sci., 2013, 48: 5410 |
| 25 | Hughes D A, Hansen N. High angle boundaries formed by grain subdivision mechanisms [J]. Acta Mater., 1997, 45: 3871 |
| 26 | Tao N R, Wang Z B, Tong W P, et al. An investigation of surface nanocrystallization mechanism in Fe induced by surface mechanical attrition treatment [J]. Acta Mater., 2002, 50: 4603 |
| 27 | Murayama M, Horita Z, Hono K. Microstructure of two-phase Al-1.7at% Cu alloy deformed by equal-channel angular pressing [J]. Acta Mater., 2001, 49: 21 |
| 28 | Liu Z Y, Liang G X, Wang E D, et al. Effect of equal-channel angular pressing on structure of Al alloy 2024 [J]. Trans. Nonferrous Met. Soc. China, 1997, 7: 160 |
| 29 | Jin X J, Chen S H, Rong L J. Microstructure modification and mechanical property improvement of reduced activation ferritic/martensitic steel by severe plastic deformation [J]. Mater. Sci. Eng., 2018, A712: 97 |
| 30 | Apps P J, Bowen J R, Prangnell P B. The effect of coarse second-phase particles on the rate of grain refinement during severe deformation processing [J]. Acta Mater., 2003, 51: 2811 |
| 31 | Huang W J. Severe plastic deformation induces Al-4wt.%Cu alloy precipitated phase re-dissolution and subsequent aging behavior [D]. Changsha: Central South University, 2012 |
| 31 | 黄文杰. 强塑性变形诱导Al-4wt.%Cu合金析出相回溶及之后的时效行为研究 [D]. 长沙: 中南大学, 2012 |
| 32 | Xu X C, Liu Z Y, Dang P, et al. Mechanism of re-dissolution and re-precipitation of second phases in Al-Zn-Mg-Cu alloy under severe plastic deformation [J]. Mater. Sci. Technol., 2005, 13: 178 |
| 32 | 许晓嫦, 刘志义, 党 朋等. 室温强塑性变形下回溶和再析出的机理研究 [J]. 材料科学与工艺, 2005, 13: 178 |
| 33 | Hu N, Xu X C, Zhang Z Z, et al. Effect of re-dissolution of severely deformed precipitated phase on mechanical properties of Al-Cu alloy [J]. Chin. J. Nonferrous Met., 2010, 20: 1922 |
| 33 | 胡 楠, 许晓嫦, 张孜昭等. 强变形诱导析出相回溶对Al-Cu合金力学性能的影响 [J]. 中国有色金属学报, 2010, 20: 1922 |
| 34 | Mao C L, Liu C X, Yu L M, et al. Mechanical properties and tensile deformation behavior of a reduced activated ferritic-martensitic (RAFM) steel at elevated temperatures [J]. Mater. Sci. Eng., 2018, A725: 283 |
| 35 | Foley D C, Hartwig K T, Maloy S A, et al. Grain refinement of T91 alloy by equal channel angular pressing [J]. J. Nucl. Mater., 2009, 389: 221 |
| 36 | Sasaki T T, Oh-Ishi K, Ohkubo T, et al. Effect of double aging and microalloying on the age hardening behavior of a Mg-Sn-Zn alloy [J]. Mater. Sci. Eng., 2011, A530: 1 |
| 37 | Panait C G, Zielińska-Lipiec A, Koziel T, et al. Evolution of dislocation density, size of subgrains and MX-type precipitates in a P91 steel during creep and during thermal ageing at 600oC for more than 100,000 h [J]. Mater. Sci. Eng., 2010, A527: 4062 |
| 38 | Hamada K, Tokuno K, Tomita Y, et al. Effects of precipitate shape on high temperature strength of modified 9Cr-1Mo steels [J]. ISIJ Int., 1995, 35: 86 |
| 39 | Ravikirana, Mythili R, Raju S, et al. Influence of W and Ta content on microstructural characteristics in heat treated 9Cr-reduced activation ferritic/martensitic steels [J]. Mater. Charact., 2013, 84: 196 |
| 40 | Brooks I, Lin P, Palumbo G, et al. Analysis of hardness-tensile strength relationships for electroformed nanocrystalline materials [J]. Mater. Sci. Eng., 2008, A491: 412 |
| 41 | Han B Q, Mohamed F A, Lavernia E J. Mechanical properties of iron processed by severe plastic deformation [J]. Metall. Mater. Trans., 2003, 34A: 71 |
| 42 | De Messemaeker J, Verlinden B, Van Humbeeck J. On the strength of boundaries in submicron IF steel [J]. Mater. Lett., 2004, 58: 3782 |
| 43 | Kashyap B P, Tangri K. Hall-Petch relationship and substructural evolution in boron containing type 316L stainless steel [J]. Acta Mater., 1997, 45: 2383 |
| 44 | Liu X D, Nagumo M, Umemoto M. The Hall-Petch relationship in nanocrystalline materials [J]. Mater. Trans., 1997, 38: 1033 |
/
| 〈 |
|
〉 |