具有异常放热现象的Fe-Nb-B-Y非晶合金燃烧机理
收稿日期: 2020-10-26
修回日期: 2020-12-02
网络出版日期: 2020-12-18
基金资助
国家自然科学基金项目(51871120);江苏省自然科学基金-杰出青年基金项目(BK20200019)
Combustion Mechanism of Fe-Nb-B-Y Amorphous Alloys with an Anomalous Exothermic Phenomenon
Received date: 2020-10-26
Revised date: 2020-12-02
Online published: 2020-12-18
Supported by
National Natural Science Foundation of China(51871120);Natural Science Foundation of Jiangsu Province-Outstanding Youth Fund Project(BK20200019)
通过同步辐射原位高能X射线衍射,结合差式扫描量热、热重分析、X射线光电子能谱等检测手段,对具有异常放热现象的铁基非晶合金条带的燃烧机理进行了系统研究。结果表明,相比不具有异常放热现象、无法自蔓延燃烧的Fe-Nb-B-Y非晶合金成分,具有异常放热现象的(Fe0.72B0.24Nb0.04)95.5Y4.5非晶条带由于快速晶化放热过程的催化,能够实现低着火点及自蔓延燃烧。与液-液相变相关联的异常放热现象诱导了升温过程中的快速晶化,并导致高温下的多步氧化反应。同时液-液相变导致高温氧化阶段的激活能降低,从而降低反应能垒,促进高温下的氧化反应。研究表明异常放热现象及其关联的液-液相变对铁基非晶合金的燃烧有“诱导活化”作用。
胡祥 , 葛嘉城 , 刘思楠 , 伏澍 , 吴桢舵 , 冯涛 , 刘冬 , 王循理 , 兰司 . 具有异常放热现象的Fe-Nb-B-Y非晶合金燃烧机理[J]. 金属学报, 2021 , 57(4) : 542 -552 . DOI: 10.11900/0412.1961.2020.00420
The functional groups in traditional energetic materials typically contain C, N, and O. These elements are usually unstable and sensitive to external stimuli. Moreover, the chemicals used during the preparation process of traditional energetic materials are toxic and pose many safety and environmental issues. As one of the metastable materials, high-energy-state amorphous alloys are potential candidates for new energetic materials with high combustion heat, low ignition temperature, non-toxicity, and improved safety. In this work, the combustion mechanism of Fe-based amorphous ribbons with an anomalous exothermic phenomenon was systematically studied using in situ synchrotron X-ray diffraction, differential scanning calorimetry, thermogravimetric analysis, and X-ray photoelectron spectroscopy. Experimental results show that compared to Fe-Nb-B-Y amorphous alloys with normal thermophysical and combustion behaviors, (Fe0.72B0.24Nb0.04)95.5Y4.5 amorphous ribbons with anomalous exothermic phenomena possess low ignition temperature and self-propagating combustion behavior due to the catalysis of the rapid crystallization exothermic process. The anomalous exothermic phenomenon and associated liquid-liquid phase transitions can cause rapid crystallization at elevated temperatures during heating, followed by multi-step oxidation. On the other hand, it was possible to significantly reduce the activation energy of high-temperature oxidation. The liquid-liquid phase transition can lower the energy barrier of the oxidation reaction. In this way, the oxidation reaction at high temperatures can be promoted. The results suggest that the liquid-liquid phase transition has an “induced activation” effect on the combustion of Fe-based amorphous alloys.
| 1 | Baletto F, Ferrando R. Structural properties of nanoclusters: Energetic, thermodynamic, and kinetic effects [J]. Rev. Mod. Phys., 2005, 77: 371 |
| 2 | Sikder A K, Sikder N. A review of advanced high performance, insensitive and thermally stable energetic materials emerging for military and space applications [J]. J. Hazard. Mater., 2004, 112: 1 |
| 3 | Li G, Zhang C Y. Review of the molecular and crystal correlations on sensitivities of energetic materials [J]. J. Hazard. Mater., 2020, 398: 122910 |
| 4 | Yu B S, Sun Y H, Bai H Y, et al. Highly energetic and flammable metallic glasses [J]. Sci. China Phys. Mech. Astron., 2020, 63: 276112 |
| 5 | Badgujar D M, Talawar M B, Asthana S N, et al. Advances in science and technology of modern energetic materials: An overview [J]. J. Hazard. Mater., 2008, 151: 289 |
| 6 | Trunov M A, Schoenitz M, Dreizin E L. Ignition of aluminum powders under different experimental conditions [J]. Propell. Explos. Pyrot., 2005, 30: 36 |
| 7 | Yagodnikov D A, Ignatov A V, Gusachenko E I. Ignition and combustion of pyrotechnic compositions based on microsized and ultra-nanosized aluminum particles in a moist medium in a two-zone gas generator [J]. Combust. Explos. Shock Waves, 2017, 53: 15 |
| 8 | Pan J, Wang Y X, Guo Q, et al. Extreme rejuvenation and softening in a bulk metallic glass [J]. Nat. Commun., 2018, 9: 560 |
| 9 | Dreizin E L. Phase changes in metal combustion [J]. Prog. Energy Combust. Sci., 2000, 26: 57 |
| 10 | Ge J C, He H Y, Zhou J, et al. In-situ scattering study of a liquid-liquid phase transition in Fe-B-Nb-Y supercooled liquids and its correlation with glass-forming ability [J]. J. Alloys Compd., 2019, 787: 831 |
| 11 | Lan S, Ren Y, Wei X Y, et al. Hidden amorphous phase and reentrant supercooled liquid in Pd-Ni-P metallic glasses [J]. Nat. Commun., 2017, 8: 14679 |
| 12 | Tanaka H. General view of a liquid-liquid phase transition [J]. Phys. Rev., 2000, 62E: 6968 |
| 13 | Palmer J C, Martelli F, Liu Y, et al. Metastable liquid-liquid transition in a molecular model of water [J]. Nature, 2014, 510: 385 |
| 14 | Shimizu R, Kobayashi M, Tanaka H. Evidence of liquid-liquid transition in triphenyl phosphite from time-resolved light scattering experiments [J]. Phys. Rev. Lett., 2014, 112: 125702 |
| 15 | Zhou Z J, Hu X, You Z, et al. Oxy-fuel combustion characteristics and kinetic parameters of lignite coal from thermo-gravimetric data [J]. Thermochim. Acta, 2013, 553: 54 |
| 16 | Fakhraai Z, Forrest J A. Measuring the surface dynamics of glassy polymers [J]. Science, 2008, 319: 600 |
| 17 | K?k M V, Acar C. Kinetics of crude oil combustion [J]. J. Therm. Anal. Calorim., 2006, 83: 445 |
| 18 | Lysenko E N, Surzhikov A P, Zhuravkov S P, et al. The oxidation kinetics study of ultrafine iron powders by thermogravimetric analysis [J]. J. Therm. Anal. Calorim., 2014, 115: 1447 |
| 19 | Qi X W, Zhou J, Yue Z X, et al. Auto-combustion synthesis of nanocrystalline LaFeO3 [J]. Mater. Chem. Phys., 2003, 78: 25 |
| 20 | Takacs L. Self-sustaining reactions induced by ball milling: An overview [J]. Int. J. Self-Propag. High-Temp. Synth., 2009, 18: 276 |
| 21 | Takahashi M, Koshimura M, Abuzuka T. Phase diagram of amorphous and crystallized Fe-B alloy system [J]. Jpn. J. Appl. Phys., 1981, 20: 1821 |
| 22 | Abrosimova G E, Aronin A S. Formation of metastable phases during crystallization of amorphous iron-based alloys [J]. Crystallogr. Rep., 2020, 65: 573 |
| 23 | Grosvenor A P, Kobe B A, Biesinger M C, et al. Investigation of multiplet splitting of Fe 2p XPS spectra and bonding in iron compounds [J]. Surf. Interface Anal., 2004, 36: 1564 |
| 24 | Yamashita T, Hayes P. Analysis of XPS spectra of Fe2+ and Fe3+ ions in oxide materials [J]. Appl. Surf. Sci., 2008, 254: 2441 |
| 25 | Kim K J, Moon D W, Lee S K, et al. Formation of a highly oriented FeO thin film by phase transition of Fe3O4 and Fe nanocrystallines [J]. Thin Solid Films, 2000, 360: 118 |
| 26 | Li Y X, Claydon J S, Ahmad E, et al. XPS and XMCD study of Fe3O4 GaAs interface [J]. IEEE Trans. Magn., 2005, 41: 2808 |
| 27 | Rydén M, Leion H, Mattisson T, et al. Combined oxides as oxygen-carrier material for chemical-looping with oxygen uncoupling [J]. Appl. Energy, 2014, 113: 1924 |
| 28 | Zhang C, Wu Y, Liu L. Robust hydrophobic Fe-based amorphous coating by thermal spraying [J]. Appl. Phys. Lett., 2012, 101: 121603 |
| 29 | Filonenko N Y, Babachenko O I, Kononenko G A. Influence of overheating and cooling rate on the structures and properties of alloys of the Fe-B system [J]. Mater. Sci., 2019, 55: 440 |
| 30 | Otero T F, Santos F. Polythiophene oxidation: Rate coefficients, activation energy and conformational energies [J]. Electrochim. Acta, 2008, 53: 3166 |
| 31 | Zhong Z Y, Highfield J, Lin M, et al. Insights into the oxidation and decomposition of CO on Au/α-Fe2O3 and on α-Fe2O3 by coupled TG-FTIR [J]. Langmuir, 2008, 24: 8576 |
| 32 | Cao C R, Lu Y M, Bai H Y, et al. High surface mobility and fast surface enhanced crystallization of metallic glass [J]. Appl. Phys. Lett., 2015, 107: 141606 |
/
| 〈 |
|
〉 |