金属学报  1983, Vol. 19 Issue (5): 95-101    
  论文 本期目录 | 过刊浏览 |
一种简单六角点阵的缺陷结构
苗柏和;孟宪英;赵伯麟
北京钢铁学院;北京钢铁学院;北京理化测试中心;北京钢铁学院
ONE KIND OF FAULT STRUCTURE OF SIMPLE HEXAGONAL LATTICE
MIAO Baihe; MENG Xianying; ZHAO Bolin (Beijing University of Iron and Steel Technology)
引用本文:

苗柏和;孟宪英;赵伯麟. 一种简单六角点阵的缺陷结构[J]. 金属学报, 1983, 19(5): 95-101.
, , . ONE KIND OF FAULT STRUCTURE OF SIMPLE HEXAGONAL LATTICE[J]. Acta Metall Sin, 1983, 19(5): 95-101.

全文: PDF(2397 KB)  
摘要: 本文使用H-700TEM双倾样品台,以μ相的α~*和[110]~*为轴旋转晶体,分别得到了一系列不同取向的倒易面衍射花样。根据衍射无系统消光现象及衍射倒易面出现的规律,可以确定GH302合金析出的μ相是简单六角点阵,a=4.75(?),c=25.8(?)。它是[001]方向有严重堆垛层错的一种缺陷结构。
Abstract:According to the facts of no systematic extinction and the sequencc of the occurrence of the reciprocal planes in a series of electron diffraction patterns obtained by tilting around the [110]~* and a~* axes of μ-phase, the lattice type of μ-phase in the superalloy GH302 has been determined tobe a simple hexagonal lattice with severe stacking faults in [001] direction and having the lattice parameters of a=4.75 (?) and c=25.8 (?).
收稿日期: 1983-05-18     
1 Arnfelt, H.; Westgren, A., Strukturbericht, 3 (1937) , 364.
2 Forsyth, J. B.; Veiga, L. M. d' Alte Da, Acta Cryst. 15 (1962) , 543.
3 Raman, A., Z. Metallk. 57 (1966) , 301.
4 Sinha, A. K.; Buckley, R. A.; Hume-Rothery, W., J. Iron Steel. Inst., 205 (1967) , 191.
5 Sinha, A. K.; Hume-Rothery, W., ibid., 205 (1967) , 1145.
6 Kohei Yagisawa; Hiroshi Fujita, Jpn. J. Appl. Phys., 6 (1967) , 826.
7 Lars Stenberg; Sten Andersson, J. Solid State Chem., 28 (1979) , 269.
8 Makoto Hirabayashi; Kenji Hiraga; Daisuke Shindo; Tadashi Yamamoto, Sci Rep. Res. Inst., Tohoku Uni. Ser. A29 Suppl. 1, (1981) , 1.
9 赵伯麟;苗柏和;陈国良,金属学报,17 (1981) ,386.
10 陈国良,谢锡善,倪克铨;徐志超;王迪,金属学报,17 (1981) ,1.
11 蔡玉林;郑运荣,金属学报,18 (1982) ,30.5