Please wait a minute...
    DOI: 10.11900/0412.1961.2025.00413
  本期目录 | 过刊浏览 |
Ti175高温钛合金中初生和次生组织的氧化差异
李晨旭, 齐萌, 孙崇昊, 张博华, 刘玉敬, 王清江, 赵焕, 刘巧沐, 赵子博
宝鸡西工钛科技股份有限公司昱华先进材料研究院项目部, 710000 中国
Differences in Oxidation between Primary and Secondary Microstructures in Ti175 High-Temperature Titanium Alloy
WANG Qing-Jiang, LIU Qiao-Mu
, Yuhua Institute of Advanced Material, Baoji Xigong Titanium Technology Co. Ltd. 710000, China
引用本文:

李晨旭, 齐萌, 孙崇昊, 张博华, 刘玉敬, 王清江, 赵焕, 刘巧沐, 赵子博. Ti175高温钛合金中初生和次生组织的氧化差异[J]. , DOI: 10.11900/0412.1961.2025.00413.
, , , , , Qing-Jiang WANG, , Qiao-Mu LIU, . Differences in Oxidation between Primary and Secondary Microstructures in Ti175 High-Temperature Titanium Alloy[J]. , , (): 0-.

全文: PDF( KB)  
摘要: 本文研究了Ti175合金在650℃高温下10 min和2 h的氧化行为,重点探讨初生与次生组织因相结构差异对氧化膜形成与演变的影响机制。结合实验表征与第一性原理计算发现:氧化10 min后,两种组织氧化行为相似,表面Ti元素氧化形成约30 nm的薄层氧化物,Al未明显参与氧化;随氧化时间延长至2 h,初生组织表面形成均匀的氧化膜,其中间形成了连续致密的Al2O3层,这显著抑制氧化速率。而次生组织因α/β相交替分布,α相形成的非连续Al2O3层无法抑制氧沿β相的快速扩散,导致氧化膜在α/β界面不均匀生长,厚度起伏较大。该研究揭示了Ti175合金中相组成与分布对氧化膜生长均匀性与抗高温氧化性能的关键作用,为优化合金微观组织设计以提高抗氧化能力提供了理论依据。
关键词 : 钛合金,Ti175,热暴露,氧化机理,第一性原理计算    
Abstract:This study investigates the oxidation behavior of Ti175 alloy at 650°C for durations of 10 minutes and 2 hours, focusing on the influence mechanism of phase structural differences between primary and secondary microstructures on the formation and evolution of the oxide film. Combining experimental characterization and first-principles calculations, it was found that after 10 minutes of oxidation, both microstructures exhibited similar oxidation behavior, with surface Ti oxidizing to form a thin oxide layer of approximately 30 nm, while Al showed no significant participation. With prolonged oxidation to 2 hours, a uniform oxide film formed on the surface of the primary microstructure, within which a continuous and dense Al2O3 layer developed in the middle, significantly inhibiting the oxidation rate. In contrast, due to the alternating distribution of α and β phases in the secondary microstructure, the discontinuous Al2O3 layer formed within the α phase could not suppress the rapid diffusion of oxygen along the β phase. This resulted in uneven growth of the oxide film at the α/β interfaces and large thickness variations. This research elucidates the critical role of phase composition and distribution in Ti175 alloy on the growth uniformity of the oxide film and its high-temperature oxidation resistance, providing a theoretical basis for optimizing alloy microstructure design to enhance oxidation resistance.
Key words: Titanium alloy, Ti175, thermal exposure, oxidation mechanism, first-principles calculation
收稿日期: 2025-12-18     
No related articles found!