Phase Field and Crystal Plasticity Simulation of Irradiation-Induced He Bubbles Evolution and Mechanical Behavior in 316H Steel and Weld Metal
Received date: 2025-08-20
Revised date: 2025-09-22
Online published: 2025-11-05
Supported by
National Funds for Distinguished Young Scholars(52025052)
316H steel is an important structural material candidate for Generation-IV advanced nuclear reactors. During service, the material operates under conditions of high temperature, irradiation, and complex stress for extended durations, and the working environment is extremely harsh. In particular, He bubbles, generated through nuclear transmutation under irradiation, can cause severe irradiation embrittlement and accelerate the failure of the material. To clarify the role of He bubbles in the degradation of 316H steel and weld metal, this study proposes a coupled computational framework that integrates the phase field model and crystal plasticity. Within this framework, the nucleation, growth, and coalescence of He bubbles in 316H steel and weld metal were simulated, and their mechanical responses were systematically analyzed. The research shows that He bubbles nucleate and grow by absorbing supersaturated vacancies and He atoms. In the later stage, they grow through coalescence and Ostwald ripening processes. As the He bubble size increases, the internal pressure gradually decreases until reaching an equilibrium state. The high density of dislocations in the weld metal, which preferentially absorb interstitial atoms, results in an increased vacancy concentration. Meanwhile, dislocations act as rapid diffusion channels. These two factors together contribute to the rapid growth of He bubbles. An increase in diffusion capacity does not change the final proportion of He bubbles; instead, it accelerates the nucleation and growth processes, thereby promoting the kinetic evolution of He bubbles in the weld metal. At small strains, the stress-strain response is governed by the effects of external strain and the internal pressure of He bubbles, with the macroscopic stress value being negative. As the external strain increases, the stress-strain response becomes influenced by the external strain. During tensile deformation, significant stress concentration arises at the He bubble-matrix interface, leading to considerable plastic deformation in these regions. At 4% applied strain, distinct plastic deformation bands form in both 316H steel and the weld metal. However, due to strain localization in the weld metal, the degree of plastic deformation is greater than that observed in 316H steel.
Key words: 316H steel; weld metal; irradiation; He bubble; phase field simulation
WANG Dong , XU Lianyong , ZHAO Lei , HAN Yongdian , SONG Kai . Phase Field and Crystal Plasticity Simulation of Irradiation-Induced He Bubbles Evolution and Mechanical Behavior in 316H Steel and Weld Metal[J]. Acta Metall Sin, 2026 , 62(1) : 173 -190 . DOI: 10.11900/0412.1961.2025.00239
| [1] | Li Y, Wang F, Zheng Y M, et al. Multiaxial isothermal and thermomechanical fatigue behavior of 316H stainless steel welded joint and life prediction [J]. Int. J. Fatigue, 2026, 203: 109295 |
| [2] | Gu Z M, Zhong M, Gong Y, et al. Tracking martensitic substructure evolution in the heat-affected zone of P91 steel: Integrating CSLM observation and post-mortem microstructural analysis [J]. Metall. Mater. Trans., 2025, 56A: 4744 |
| [3] | Lin Y R, Chen W Y, Tan L Z, et al. Bubble formation in helium-implanted nanostructured ferritic alloys at elevated temperatures [J]. Acta Mater., 2021, 217: 117165 |
| [4] | Li J T, Beyerlein I J, Han W Z. Helium irradiation-induced ultrahigh hardening in niobium [J]. Acta Mater., 2022, 226: 117656 |
| [5] | Jublot-Leclerc S, Lescoat M L, Fortuna F, et al. TEM study of the nucleation of bubbles induced by He implantation in 316L industrial austenitic stainless steel [J]. J. Nucl. Mater., 2015, 466: 646 |
| [6] | Chen Y, Li Y P, Ran G, et al. In-situ TEM observation of the evolution of dislocation loops and helium bubbles in a pre helium irradiated FeCrAl alloy during annealing [J]. Prog. Nucl. Energy, 2020, 129: 103502 |
| [7] | Villacampa I, Chen J C, Sp?tig P, et al. Helium bubble evolution and hardening in 316L by post-implantation annealing [J]. J. Nucl. Mater., 2018, 500: 389 |
| [8] | Judge C D, Gauquelin N, Walters L, et al. Intergranular fracture in irradiated Inconel X-750 containing very high concentrations of helium and hydrogen [J]. J. Nucl. Mater., 2015, 457: 165 |
| [9] | Miura T, Fujii K, Fukuya K. Micro-mechanical investigation for effects of helium on grain boundary fracture of austenitic stainless steel [J]. J. Nucl. Mater., 2015, 457: 279 |
| [10] | Fu C L, Li J J, Bai J J, et al. Evolution of helium bubbles in SLM 316L stainless steel irradiated with helium ions at different temperatures [J]. J. Nucl. Mater., 2022, 562: 153609 |
| [11] | Bai J J, Li J J, Fu C L, et al. Effect of He ion irradiation on the GH3535 weld metal at high temperature [J]. Acta Metall. Sin., 2024, 60: 299 |
| 白菊菊, 李健健, 付崇龙 等. GH3535合金焊缝高温氦离子辐照效应 [J]. 金属学报, 2024, 60: 299 | |
| [12] | Wang D, Xu L Y, Zhao L, et al. Microstructural and mechanical responses of 316H and weld metal under Helium irradiation at 550 oC [J]. J. Nucl. Mater., 2025, 605: 155564 |
| [13] | Jelea A. Molecular dynamics modeling of helium bubbles in austenitic steels [J]. Nucl. Instrum. Methods Phys. Res. Sect., 2018, 425B: 50 |
| [14] | Stan M, Ramirez J C, Cristea P, et al. Models and simulations of nuclear fuel materials properties [J]. J. Alloys Compd., 2007, 444-445: 415 |
| [15] | Hu S Y, Henager Jr C H, Heinisch H L, et al. Phase-field modeling of gas bubbles and thermal conductivity evolution in nuclear fuels [J]. J. Nucl. Mater., 2009, 392: 292 |
| [16] | Millett P C, El-Azab A, Rokkam S, et al. Phase-field simulation of irradiated metals: Part I: Void kinetics [J]. Comput. Mater. Sci., 2011, 50: 949 |
| [17] | Millett P C, El-Azab A, Wolf D. Phase-field simulation of irradiated metals: Part II: Gas bubble kinetics [J]. Comput. Mater. Sci., 2011, 50: 960 |
| [18] | Li Y L, Hu S Y, Montgomery R, et al. Phase-field simulations of intragranular fission gas bubble evolution in UO2 under post-irradiation thermal annealing [J]. Nucl. Instrum. Methods Phys. Res. Sect., 2013, 303B: 62 |
| [19] | Hu S Y, Burkes D E, Lavender C A, et al. Formation mechanism of gas bubble superlattice in UMo metal fuels: Phase-field modeling investigation [J]. J. Nucl. Mater., 2016, 479: 202 |
| [20] | Liang L Y, Mei Z G, Soo Kim Y, et al. Three-dimensional phase-field simulations of intragranular gas bubble evolution in irradiated U-Mo fuel [J]. Comput. Mater. Sci., 2018, 145: 86 |
| [21] | Jiang Y B, Sun Z P, Wang D J, et al. Effects of grain boundaries on the evolution of radiation-induced bubbles in polycrystalline tungsten: A phase-field simulation [J]. J. Nucl. Mater., 2024, 588: 154757 |
| [22] | Liu C Y, Feng Z H, Zhang Y P, et al. Phase field simulation of bubble evolution dynamics in Fe-Cr alloys [J]. Acta Metall. Sin., 2024, 60: 1279 |
| 刘彩艳, 冯泽华, 张云鹏 等. Fe-Cr合金气泡演化动力学的相场法模拟 [J]. 金属学报, 2024, 60: 1279 | |
| [23] | Hu S Y, Beeler B. Gas bubble evolution in polycrystalline UMo fuels under elastic-plastic deformation: A phase-field model with crystal-plasticity [J]. Front. Mater., 2021, 8: 682667 |
| [24] | Demir E, Horton E W, Mokhtarishirazabad M, et al. Grain size and shape dependent crystal plasticity finite element model and its application to electron beam welded SS316L [J]. J. Mech. Phys. Solids, 2023, 178: 105331 |
| [25] | Gan L F, Zhu B Y, Ling C, et al. Micro-mechanics investigation of heterogeneous deformation fields and crack initiation driven by the local stored energy density in austenitic stainless steel welded joints [J]. J. Mech. Phys. Solids, 2024, 188: 105652 |
| [26] | Jiang H, Yang Z Y, Guo Z F, et al. Interpretation of mechanical properties gradient in laser-welded joints: Experiments and grain morphology-dependent crystal plasticity modeling [J]. J. Mater. Res. Technol., 2024, 33: 5934 |
| [27] | Wang D, Zhao L, Xu L Y, et al. A microstructure-based study of irradiation hardening in stainless steel: Experiment and phase field modeling [J]. J. Nucl. Mater., 2022, 569: 153940 |
| [28] | Xiao Z H, Wang Y F, Hu S Y, et al. A quantitative phase-field model of gas bubble evolution in UO2 [J]. Comput. Mater. Sci., 2020, 184: 109867 |
| [29] | Jiang Y B, Xin Y, Liu W B, et al. Phase-field simulation of radiation-induced bubble evolution in recrystallized U-Mo alloy [J]. Nucl. Eng. Technol., 2022, 54: 226 |
| [30] | Wang Y F, Xiao Z H, Hu S Y, et al. A phase field study of the thermal migration of gas bubbles in UO2 nuclear fuel under temperature gradient [J]. Comput. Mater. Sci., 2020, 183: 109817 |
| [31] | Wang Y F, Xiao Z H, Shi S Q. Xe gas bubbles evolution in UO2 fuels—A phase field simulation [J]. Sci. Sin. Phys. Mech. Astron., 2019, 49: 114607 |
| 王亚峰, 肖知华, 石三强. UO2核燃料中Xe气泡演化的相场模型与分析 [J]. 中国科学: 物理学 力学 天文学, 2019, 49: 114607 | |
| [32] | Magomedov M N. Parameters of the vacancy formation and self-diffusion in the iron [J]. J. Phys. Chem. Solids, 2023, 172: 111084 |
| [33] | Wen P, Tonks M R, Phillpot S R, et al. The effect of stress on the migration of He gas bubbles under a thermal gradient in Fe by phase-field modeling [J]. Comput. Mater. Sci., 2022, 209: 111392 |
| [34] | Caro A, Schwen D, Hetherly J, et al. The capillarity equation at the nanoscale: Gas bubbles in metals [J]. Acta Mater., 2015, 89: 14 |
| [35] | Khachaturyan A G. Theory of Structural Transformations in Solids [M]. New York: John Wiley Sons, 1983: 201 |
| [36] | Jiang W, Hu T C, Aagesen L K, et al. Three-dimensional phase-field modeling of porosity dependent intergranular fracture in UO2 [J]. Comput. Mater. Sci., 2020, 171: 109269 |
| [37] | Li Y L, Hu S Y, Barker E, et al. Effect of grain structure and strain rate on dynamic recrystallization and deformation behavior: A phase field-crystal plasticity model [J]. Comput. Mater. Sci., 2020, 180: 109707 |
| [38] | Demir E, Martinez-Pechero A, Hardie C, et al. OXFORD-UMAT: An efficient and versatile crystal plasticity framework [J]. Int. J. Solids Struct., 2025, 307: 113110 |
| [39] | Monnet G, Mai C. Prediction of irradiation hardening in austenitic stainless steels: Analytical and crystal plasticity studies [J]. J. Nucl. Mater., 2019, 518: 316 |
| [40] | Kubin L, Devincre B, Hoc T. Modeling dislocation storage rates and mean free paths in face-centered cubic crystals [J]. Acta Mater., 2008, 56: 6040 |
| [41] | Patra A, McDowell D L. Crystal plasticity-based constitutive modelling of irradiated bcc structures [J]. Philos. Mag., 2012, 92: 861 |
| [42] | Cahn J W, Hilliard J E. Free energy of a nonuniform system. I. Interfacial free energy [J]. J. Chem. Phys., 1958, 28: 258 |
| [43] | Cahn J W. On spinodal decomposition [J]. Acta Metall., 1961, 9: 795 |
| [44] | Cahn J W, Allen S M. A microscopic theory for domain wall motion and its experimental verification in Fe-Al alloy domain growth kinetics [J]. J. Phys. Colloq., 1977, 38: C7-51 |
| [45] | Jokisaari A M, Permann C, Thornton K. A nucleation algorithm for the coupled conserved-nonconserved phase field model [J]. Comput. Mater. Sci., 2016, 112: 128 |
| [46] | Aagesen L K, Jokisaari A, Schwen D, et al. A phase-field model for void and gas bubble superlattice formation in irradiated solids [J]. Comput. Mater. Sci., 2022, 215: 111772 |
| [47] | Chen L Q, Shen J. Applications of semi-implicit Fourier-spectral method to phase field equations [J]. Comput. Phys. Commun., 1998, 108: 147 |
| [48] | Moulinec H, Suquet P. A numerical method for computing the overall response of nonlinear composites with complex microstructure [J]. Comput. Methods Appl. Mech. Eng., 1998, 157: 69 |
| [49] | Lebensohn R A, Kanjarla A K, Eisenlohr P. An elasto-viscoplastic formulation based on fast Fourier transforms for the prediction of micromechanical fields in polycrystalline materials [J]. Int. J. Plast., 2012, 32-33: 59 |
| [50] | Aagesen L K, Schwen D, Tonks M R, et al. Phase-field modeling of fission gas bubble growth on grain boundaries and triple junctions in UO2 nuclear fuel [J]. Comput. Mater. Sci., 2019, 161: 35 |
| [51] | Kohnert A A, Capolungo L. The kinetics of static recovery by dislocation climb [J]. npj Comput. Mater., 2022, 8: 104 |
| [52] | Stechauner G, Kozeschnik E. Self-diffusion in grain boundaries and dislocation pipes in Al, Fe, and Ni and application to AlN precipitation in steel [J]. J. Mater. Eng. Perform., 2014, 23: 1576 |
| [53] | Chen W B, Ding X B, Zhai L H, et al. Effect of δ-ferrite decomposition on the tensile properties of one modified 316H stainless steel: Experimental investigations and crystal plastic finite element simulations [J]. Mater. Sci. Eng., 2024, A915: 147224 |
| [54] | Sedighiani K, Diehl M, Traka K, et al. An efficient and robust approach to determine material parameters of crystal plasticity constitutive laws from macro-scale stress-strain curves [J]. Int. J. Plast., 2020, 134: 102779 |
| [55] | Schroeder H, Fichtner P F P. On the coarsening mechanisms of helium bubbles—Ostwald ripening versus migration and coalescence [J]. J. Nucl. Mater., 1991, 179-181: 1007 |
| [56] | Ding X J, Zhao J J, Huang H, et al. Effect of damage rate on the kinetics of void nucleation and growth by phase field modeling for materials under irradiations [J]. J. Nucl. Mater., 2016, 480: 120 |
| [57] | Stoller R E, Osetsky Y N. An atomistic assessment of helium behavior in iron [J]. J. Nucl. Mater., 2014, 455: 258 |
| [58] | Sun T Y, Niu T J, Shang Z X, et al. An in situ study on the effect of grain boundaries on helium bubble formation in dual beam irradiated FeCrAl alloy [J]. Acta Mater., 2023, 245: 118613 |
| [59] | Pavan A R, Sakthivel T, Arivazhagan B, et al. A comparative study on the microstructural evolution and mechanical behavior of 316LN stainless steel welds made using hot-wire tungsten inert gas and activated tungsten inert gas process [J]. J. Mater. Eng. Perform., 2024, 33: 13618 |
| [60] | Patra A, McDowell D L. Crystal plasticity investigation of the microstructural factors influencing dislocation channeling in a model irradiated bcc material [J]. Acta Mater., 2016, 110: 364 |
/
| 〈 |
|
〉 |