Research paper

Corrosion and Cavitation Erosion Resistance of 316L Stainless Steels Produced by Laser Metal Deposition

  • JIANG Huazhen ,
  • PENG Shuang ,
  • HU Qiyun ,
  • WANG Guangyi ,
  • CHEN Qisheng ,
  • LI Zhengyang ,
  • SUN Huilei ,
  • FANG Jiahuiyu
Expand
  • 1 Wide Field Flight Engineering Science and Application Center, Institute of Mechanics, Chinese Academy of Sciences, Beijing 100190, China
    2 Collage of Materials Science and Technology, Nanjing University of Aeronautics and Astronautics, Nanjing 210016, China
    3 School of Engineering Science, University of Chinese Academy of Sciences, Beijing 100049, China
    4 School of Mechanical Engineering, Hebei University of Science and Technology, Shijiazhuang 050018, China
CHEN Qisheng, professor, Tel: (010)82544092, E-mail: qschen@imech.ac.cn;
LI Zhengyang, associate professor, Tel: (010)82544258, E-mail: zyli@imech.ac.cn

Received date: 2022-08-15

  Revised date: 2022-09-22

  Online published: 2023-01-10

Supported by

National Natural Science Foundation of China(11772344)

Abstract

Corrosion and cavitation erosion are important indicators for evaluating the performance and reliability of hydraulic machinery. Laser metal deposition (LMD), as an important technique for both surface modification and complex component fabrication, is proven to be effective in enhancing the mechanical properties of materials. In this study, 316L stainless steel (316L SS) samples were fabricated using LMD and the effects of laser power, scanning strategy, surface remelting, and build direction on the electrochemical corrosion and cavitation erosion resistance of the LMD-produced samples were systematically studied. The obtained results were compared with those of a wrought counterpart. The corrosion resistance of the LMD-produced samples in a 3.5%NaCl solution was tested via open-circuit potential measurement and potentiodynamic polarization tests. Also, the cavitation erosion resistance of the LMD-produced samples was studied according to different process parameters. The microstructure of the forged 316L SS sample was characterized with uniformly distributed equiaxed grains, whereas the LMD-produced samples exhibited a process-dependent nonequilibrium microstructure consisting of high-/low-angle grain boundaries, tortuous grains, cellular/dendritic substructures, and processing-related defects. The grain size of the LMD-produced 316L SS sample was much larger than that of the forged 316L SS. By increasing the laser power or changing the sample from horizontally built to vertically built, both the grain size and dendritic arm spacing of the material tended to increase. However, when surface remelting and the 90°-rotation scanning strategy were adopted, the changes in the grain size and dendritic arm spacing of the material were obviously different. Results of a microhardness test showed that the dendritic arm spacing can better match the microhardness evolution than the grain size. This microstructural difference also led to a significantly different electrochemical corrosion and cavitation erosion performance from that of the forged 316L SS. Results of an electrochemical corrosion test showed that the corrosion resistance of the LMD-produced 316L SS sample was much better than that of the forged 316L SS, i.e., the polarization resistance (Rp) of the LMD-produced 316L SS sample under different processing increased by about 2-98 times, while the corrosion current density (icorr) decreased by one to two orders of magnitude. The test results of an ultrasonic vibration cavitation system showed that the cavitation erosion resistance of the LMD-produced 316L SS sample was better than that of the forged 316L SS. However, stress concentration may be induced in local areas such as pores and grain boundaries, which, in turn, facilitate preferentially cavitation damage in these areas. Also, protrusion topography appeared, and gradually disappeared to form a large number of dimples in the subsequent cavitation erosion process. The cavitation erosion resistance of the material mainly depended on its local mechanical properties. The microhardness test results showed that the hardness of the LMD-produced 316L SS sample was significantly higher than that of the forged sample, so its cavitation erosion resistance was significantly improved. However, because of the heterogeneous microstructure and process-related pore defects formed in the LMD-produced samples, the microhardness contour exhibited a spatially nonuniform distribution characteristic; hence, the surface morphology of the LMD-produced 316L SS sample was seriously eroded in some local areas after cavitation.

Cite this article

JIANG Huazhen , PENG Shuang , HU Qiyun , WANG Guangyi , CHEN Qisheng , LI Zhengyang , SUN Huilei , FANG Jiahuiyu . Corrosion and Cavitation Erosion Resistance of 316L Stainless Steels Produced by Laser Metal Deposition[J]. Acta Metall Sin, 2024 , 60(11) : 1512 -1530 . DOI: 10.11900/0412.1961.2022.00382

References

1 Park I C,Kim S J. Cavitation erosion behavior in seawater of electroless Ni-P coating and process optimization using Taguchi method [J]. Appl. Surf. Sci., 2019, 477: 37
2 Xu J, Peng S, Li Z Y, et al. The influence of semiconducting properties of passive films on the cavitation erosion resistance of a NbN nanoceramic coating [J]. Ultrason. Sonochem., 2021, 71: 105406
3 Hardes C, P?hl F, R?ttger A, et al. Cavitation erosion resistance of 316L austenitic steel processed by selective laser melting (SLM) [J]. Addit. Manuf., 2019, 29: 100786
4 Li Z, Voisin T, McKeown J T, et al. Tensile properties, strain rate sensitivity, and activation volume of additively manufactured 316L stainless steels [J]. Int. J. Plast., 2019, 120: 395
5 Zhong Y, Liu L F, Wikman S, et al. Intragranular cellular segregation network structure strengthening 316L stainless steel prepared by selective laser melting [J]. J. Nucl. Mater., 2016, 470: 170
6 Kong D C, Ni X Q, Dong C F, et al. Heat treatment effect on the microstructure and corrosion behavior of 316L stainless steel fabricated by selective laser melting for proton exchange membrane fuel cells [J]. Electrochim. Acta, 2018, 276: 293
7 Jiang H Z, Fang J H Y, Chen Q S, et al. State of the art of selective laser melted 316L stainless steel: Process, microstructure, and mechanical properties [J]. Chin. J. Lasers, 2022, 49: 1402804
  蒋华臻, 房佳汇钰, 陈启生 等. 激光选区熔化成形316L不锈钢工艺、微观组织、力学性能的研究现状 [J]. 中国激光, 2022, 49: 1402804
8 Ma M M, Wang Z M, Zeng X Y. A comparison on metallurgical behaviors of 316L stainless steel by selective laser melting and laser cladding deposition [J]. Mater. Sci. Eng., 2017, A685: 265
9 Jiang H Z, Li Z Y, Feng T, et al. Effect of process parameters on defects, melt pool shape, microstructure, and tensile behavior of 316L stainless steel produced by selective laser melting [J]. Acta Metall. Sin. (Engl. Lett.), 2021, 34: ? 495
10 Wang Y M, Voisin T, McKeown J T, et al. Additively manufactured hierarchical stainless steels with high strength and ductility [J]. Nat. Mater., 2018, 17: 63
11 Saboori A, Aversa A, Marchese G, et al. Microstructure and mechanical properties of AISI 316L produced by directed energy deposition-based additive manufacturing: A review [J]. Appl. Sci., 2020, 10: 3310
12 Herzog D, Seyda V, Wycisk E, et al. Additive manufacturing of metals [J]. Acta Mater., 2016, 117: 371
13 Liu L F, Ding Q Q, Zhong Y, et al. Dislocation network in additive manufactured steel breaks strength-ductility trade-off [J]. Mater. Today, 2018, 21: 354
14 Shamsujjoha M, Agnew S R, Fitz-Gerald J M, et al. High strength and ductility of additively manufactured 316L stainless steel explained [J]. Metall. Mater. Trans., 2018, 49A: 3011
15 Kong D C, Dong C F, Ni X Q, et al. Mechanical properties and corrosion behavior of selective laser melted 316L stainless steel after different heat treatment processes [J]. J. Mater. Sci. Technol., 2019, 35: 1499
16 Zi?tala M, Durejko T, Polański M, et al. The microstructure, mechanical properties and corrosion resistance of 316L stainless steel fabricated using laser engineered net shaping [J]. Mater. Sci. Eng., 2016, A677: 1
17 Yan Z, Zou K, Cheng M P, et al. Revealing relationships between heterogeneous microstructure and strengthening mechanism of austenitic stainless steels fabricated by directed energy deposition (DED) [J]. J. Mater. Res. Technol., 2021, 15: 582
18 Guo P, Zou B, Huang C Z, et al. Study on microstructure, mechanical properties and machinability of efficiently additive manufactured AISI 316L stainless steel by high-power direct laser deposition [J]. J. Mater. Sci. Technol., 2017, 240: 12
19 Yang N, Yee J, Zheng B, et al. Process-structure-property relationships for 316L stainless steel fabricated by additive manufacturing and its implication for component engineering [J]. J. Therm. Spray Technol., 2017, 26: 610
20 Aversa A, Marchese G, Bassini E. Directed energy deposition of AISI 316L stainless steel powder: Effect of process parameters [J]. Metals, 2021, 11: 932
21 Ding H Q, Tang Q, Zhu Y, et al. Cavitation erosion resistance of 316L stainless steel fabricated using selective laser melting [J]. Friction, 2021, 9: 1580
22 Zhu Y, Yang Y, Lu P, et al. Influence of surface pores on selective laser melted parts under lubricated contacts: A case study of a hydraulic spool valve [J]. Virtual Phys. Prototy., 2019, 14: 395
23 Sprouster D J, Cunningham W S, Halada G P, et al. Dislocation microstructure and its influence on corrosion behavior in laser additively manufactured 316L stainless steel [J]. Addit. Manuf., 2021, 47: 102263
24 Kazemipour M, Mohammadi M, Mfoumou E, et al. Microstructure and corrosion characteristics of selective laser-melted 316L stainless steel: The impact of process-induced porosities [J]. JOM, 2019, 71: 3230
25 Nie J J, Wei L, Jiang Y, et al. Corrosion mechanism of additively manufactured 316?L stainless steel in 3.5?wt.% NaCl solution [J]. Mater. Today Commun., 2021, 26: 101648
26 Hou J Y, Li Z Y, Jiang H Z, et al. Process and properties of Ti6Al4V manufactured using laser melting deposition with dimensionless processing diagram [J]. Chin. J. Lasers, 2022, 49: 0202013
  候静宇, 李正阳, 蒋华臻 等. 基于无量纲工艺图的激光熔化沉积制备Ti6Al4V工艺与性能研究 [J]. 中国激光, 2022, 49: 0202013
27 Jiang H Z, Li Z Y, Feng T, et al. Factor analysis of selective laser melting process parameters with normalised quantities and Taguchi method [J]. Opt. Laser Technol., 2019, 119: 105592
28 Jiang H Z, Li Z Y, Feng T, et al. Effect of annealing temperature and strain rate on mechanical property of a selective laser melted 316L stainless steel [J]. Acta Metall. Sin. (Engl. Lett.), 2022, 35: 773
29 Lu K, Lu L, Suresh S. Strengthening materials by engineering coherent internal boundaries at the nanoscale [J]. Science, 2009, 324: 349
30 Khodabakhshi F, Farshidianfar M H, Gerlich A P, et al. Microstructure, strain-rate sensitivity, work hardening, and fracture behavior of laser additive manufactured austenitic and martensitic stainless steel structures [J]. Mater. Sci. Eng., 2019, A756: 545
31 Sun Z J, Tan X P, Tor S B, et al. Simultaneously enhanced strength and ductility for 3D-printed stainless steel 316L by selective laser melting [J]. NPG Asia Mater., 2018, 10: 127
32 Ion J C, Shercliff H R, Ashby M F. Diagrams for laser materials processing [J]. Acta Metall. Mater., 1992, 40: 1539
33 Kamath C, El-dasher B, Gallegos G F, et al. Density of additively-manufactured, 316L SS parts using laser powder-bed fusion at powers up to 400 W [J]. Int. J. Adv. Manuf. Technol., 2014, 74: 65
34 Yu W H, Sing S L, Chua C K, et al. Influence of re-melting on surface roughness and porosity of AlSi10Mg parts fabricated by selective laser melting [J]. J. Alloys Compd., 2019, 792: 574
35 Kim T H, Baek G Y, Jeon J B, et al. Effect of laser rescanning on microstructure and mechanical properties of direct energy deposited AISI 316L stainless steel [J]. Surf. Coat. Technol., 2021, 405: 126540
36 Saboori A, Piscopo G, Lai M, et al. An investigation on the effect of deposition pattern on the microstructure, mechanical properties and residual stress of 316L produced by directed energy deposition [J]. Mater. Sci. Eng., 2020, A780: 139179
37 Ronneberg T, Davies C M, Hooper P A. Revealing relationships between porosity, microstructure and mechanical properties of laser powder bed fusion 316L stainless steel through heat treatment [J]. Mater. Des., 2020, 189: 108481
38 Casati R, Lemke J, Vedani M. Microstructure and fracture behavior of 316L austenitic stainless steel produced by selective laser melting [J]. J. Mater. Sci. Technol., 2016, 32: 738
39 Yu C F, Zhong Y, Zhang P, et al. Effect of build direction on fatigue performance of L-PBF 316L stainless steel [J]. Acta Metall. Sin. (Engl. Lett.), 2020, 33: 539
40 Güden M, Yava? H, Tanr?kulu A A, et al. Orientation dependent tensile properties of a selective-laser-melt 316L stainless steel [J]. Mater. Sci. Eng., 2021, A824: 141808
41 Shiau C H, McMurtrey M D, O'Brien R C, et al. Deformation behavior and irradiation tolerance of 316 L stainless steel fabricated by direct energy deposition [J]. Mater. Des., 2021, 204: 109644
42 Zhang K, Wang S J, Liu W J, et al. Characterization of stainless steel parts by laser metal deposition shaping [J]. Mater. Des., 2014, 55: 104
43 Katayama S, Matsunawa A. Solidification microstructure of laser welded stainless steels [J]. ICALEO, 1984, 1984: 60
44 Ren J, Mahajan C, Liu L, et al. Corrosion behavior of selectively laser melted CoCrFeMnNi high entropy alloy [J]. Metals, 2019, 9: 1029
45 Salman O O, Gammer C, Chaubey A K, et al. Effect of heat treatment on microstructure and mechanical properties of 316L steel synthesized by selective laser melting [J]. Mater. Sci. Eng., 2019, A748: 205
46 Montero-Sistiaga M L, Godino-Martinez M, Boschmans K, et al. Microstructure evolution of 316L produced by HP-SLM (high power selective laser melting) [J]. Addit. Manuf., 2018, 23: 402
47 Wang D, Song C H, Yang Y Q, et al. Investigation of crystal growth mechanism during selective laser melting and mechanical property characterization of 316L stainless steel parts [J]. Mater. Des., 2016, 100: 291
48 Krakhmalev P, Fredriksson G, Svensson K, et al. Microstructure, solidification texture, and thermal stability of 316 L stainless steel manufactured by laser powder bed fusion [J]. Metals, 2018, 8: 643
49 Li Z, He B, Guo Q. Strengthening and hardening mechanisms of additively manufactured stainless steels: The role of cell sizes [J]. Scr. Mater., 2020, 177: 17
50 Wang P, Goh M H, Li Q, et al. Effect of defects and specimen size with rectangular cross-section on the tensile properties of additively manufactured components [J]. Virtual Phys. Prototy., 2020, 15: 251
51 Zheng Z B, Long J, Wang S, et al. Cavitation erosion-corrosion behaviour of Fe-10Cr martensitic steel microalloyed with Zr in 3.5% NaCl solution [J]. Corros. Sci., 2021, 184: 109382
52 Cherry J A, Davies H M, Mehmood S, et al. Investigation into the effect of process parameters on microstructural and physical properties of 316L stainless steel parts by selective laser melting [J]. Int. J. Adv. Manuf. Technol., 2015, 76: 869
53 Stout K J, Blunt L. Three Dimensional Surface Topography [M]. 2nd Ed., London: Kogan Page Ltd., 2000: 157
Outlines

/