Research paper

Effect of Pre-Oxidation Treatment on the Corrosion Resistance in Stagnant Liquid Pb-Bi Eutectic of 12Cr Ferritic/Martensitic Steel

  • PAN Xia ,
  • ZHANG Yangpeng ,
  • DONG Zhihong ,
  • CHEN Shenghu ,
  • JIANG Haichang ,
  • RONG Lijian
Expand
  • 1 Institute of Metal Research, Chinese Academy of Sciences, Shenyang 110016, China
    2 School of Materials Science and Engineering, University of Science and Technology of China, Shenyang 110016, China
    3 CAS Key Laboratory of Nuclear Materials and Safety Assessment, Institute of Metal Research, Chinese Academy of Sciences, Shenyang 110016, China
ZHANG Yangpeng, associate professor, Tel: (024)23971985, E-mail: ypzhang@imr.ac.cn

Received date: 2022-05-31

  Revised date: 2022-08-03

  Online published: 2022-09-08

Supported by

National Natural Science Foundation of China(51871218);Doctoral Start-up Project of Liaoning Province Natural Science Foundation(2020-BS-006)

Abstract

Lead-cooled fast reactors using liquid lead or lead-bismuth eutectic (LBE) alloy coolants have attracted international attention due to their unique advantages in safety, economy, and sustainable development. The availability of suitable core materials is one of the key challenges restricting the development and application of the lead-cooled fast reactor technology. Ferritic/martensitic steel is one of the important candidates for nuclear reactor fuel cladding, but the dissolution of Cr and Ni occurs in it upon contact with high-temperature LBE, resulting in cladding failure. Adding Si can improve corrosion resistance, and based on this property, previous work developed a high-Si ferritic/martensitic steel for LBE alloy-cooled fast reactor. Recently, pre-oxidation treatment was proposed to further improve the corrosion performance of steel in contact with LBE. However, the structure of the oxide film formed after the pre-oxidation of 12Cr ferritic/martensitic steel, the effect on corrosion resistance, and the failure mechanism are not clear. In this study, a pre-oxidized film was formed on the steel surface and its structure was characterized. Steel corrosion experiments using oxygen-saturated LBE at 550oC were also performed to analyze the influence of pre-oxidation treatment on the LBE alloy coolant corrosion resistance of steel. The results demonstrated that the oxide films formed when steel is pre-oxidized at 720oC in 1%O2 + 99%N2 atmosphere for 1 h are mainly (Fe, Cr)2O3 and MnCr2O4 oxides. The oxide films can effectively prevent the outward diffusion of Fe in steel and the inward diffusion of O in LBE, thereby improving the corrosion resistance of steel to stagnant oxygen-saturated LBE alloy coolant at 550oC. However, due to the high diffusion rate of Mn and its high solubility in LBE alloys, the Mn in the pre-oxidized film will gradually diffuse and dissolve into the LBE alloy, rendering subsequently a part of the oxide film ineffective and forming a localized corrosion zone. After 1000 h of Pb-Bi corrosion, the local corrosion area on the alloy surface can reach 60%. This study revealed the microstructure, protective effect, and failure mechanism of the pre-oxidized film on the surface of high-Si ferritic/martensitic steel, and suggested research directions for further improving the effectiveness and stability of the pre-oxidized film.

Cite this article

PAN Xia , ZHANG Yangpeng , DONG Zhihong , CHEN Shenghu , JIANG Haichang , RONG Lijian . Effect of Pre-Oxidation Treatment on the Corrosion Resistance in Stagnant Liquid Pb-Bi Eutectic of 12Cr Ferritic/Martensitic Steel[J]. Acta Metall Sin, 2024 , 60(5) : 639 -649 . DOI: 10.11900/0412.1961.2022.00267

References

1 Yvon P. Structural Materials for Generation IV Nuclear Reactors[M]. Amsterdam: Woodhead Publishing, 2017: 651
2 OECD/NEA Nuclear Science Committee, translated by Rong L J, Zhang Y T, Lu S P, et al. Handbook on Lead-Bismuth Eutectic Alloy and Lead: Properties, Materials Compatibility, Thermalhydraulics and Technologies[M]. Beijing: Science Press, 2007: 3
  OECD/NEA Nuclear Science Committee著, 戎利建, 张玉妥, 陆善平等译. 铅与铅铋共晶合金手册——性能、材料相容性、热工水力学和技术[M]. 北京: 科学出版社, 2007: 3
3 Alemberti A, Smirnov V, Smith C F, et al. Overview of lead-cooled fast reactor activities[J]. Prog. Nucl. Energy, 2014, 77: 300
4 Alemberti A. The lead fast reactor: An opportunity for the future?[J]. Engineering, 2016, 2: 59
5 Tian S J, Zhang J W. Corrosion behavior of 316L and T91 steels in stagnant lead-bismuth eutectic at 550oC[J]. J. Univ. Sci. Technol. China, 2015, 45: 751
  田书建, 张建武. 316L和T91不锈钢在550℃静态铅铋合金中的腐蚀行为[J]. 中国科学技术大学学报, 2015, 45: 751
6 Eliseeva O I, Tsisar V P. Effect of temperature on the interaction of éP823 steel with lead melts saturated with oxygen[J]. Mater. Sci., 2007, 43: 230
7 Yang K, Yan W, Wang Z G, et al. Development of a novel structural material (SIMP steel) for nuclear equipment with balanced resistances to high temperature, radiation and liquid metal corrosion[J]. Acta Metall. Sin., 2016, 52: 1207
  杨 柯, 严 伟, 王志光 等. 核用新型耐高温、抗辐照、耐液态金属腐蚀结构材料——SIMP钢的研究进展[J]. 金属学报, 2016, 52: 1207
8 Lu Y H, Song Y Y, Chen S H, et al. Effects of Al and Si on mechanical properties and corrosion resistance in liquid Pb-Bi eutectic of 9Cr2WVTa steel[J]. Acta Metall. Sin., 2016, 52: 298
  鲁艳红, 宋元元, 陈胜虎 等. Al和Si对9Cr2WVTa钢力学性能及耐Pb-Bi腐蚀性能的影响[J]. 金属学报, 2016, 52: 298
9 Yang H Y, Zhang Y P, Xu H T, et al. A kind of high-silicon and high-chromium ferritic/martensitic heat-resistant steel resistant to liquid lead or lead-bismuth corrosion and preparation method thereof[P]. Chin Pat, 202110724403.0, 2021
  杨红义, 张洋鹏, 徐海涛 等. 一种耐液态铅或铅铋腐蚀高硅高铬铁素体/马氏体耐热钢及其制备方法[P]. 中国专利, 202110724403.0, 2021
10 Chen S H, Rong L J. Effect of silicon on the microstructure and mechanical properties of reduced activation ferritic/martensitic steel[J]. J. Nucl. Mater., 2015, 459: 13
11 Wang J, Lu S P, Rong L J, et al. Effect of silicon contents on the microstructures and mechanical properties of heat affected zones for 9Cr2WVTa steels[J]. J. Nucl. Mater., 2016, 470: 1
12 Yaskiv O I, Kukhar I S, Fedirko V M. Effect of preliminary diffusion oxidation on mechanical properties of ferritic steel in oxygen-containing lead[J]. Fusion Eng. Des., 2015, 101: 134
13 Lillard R S, Valot C, Hill M A, et al. Influence of preoxidation on the corrosion of steels in liquid lead-bismuth eutectic[J]. Corrosion, 2004, 60: 1031
14 Xu S, Long F, Persaud S Y, et al. Oxidation behavior of 9Cr-4.5Al ODS steel in 600oC supercritical water and the effect of pre-oxidation[J]. Corros. Sci., 2020, 165: 108380
15 Yas'kiv O I, Eliseeva O I, Kharkhalis A Y, et al. Influence of preliminary oxidation on the corrosion resistance of ferritic-martensitic steels in lead melts[J]. Mater. Sci., 2016, 51: 854
16 Abe F, Kutsumi H, Haruyama H, et al. Improvement of oxidation resistance of 9 mass% chromium steel for advanced-ultra supercritical power plant boilers by pre-oxidation treatment[J]. Corros. Sci., 2017, 114: 1
17 Lehmusto J, Lindberg D, Yrjas P, et al. The effect of temperature on the formation of oxide scales regarding commercial superheater steels[J]. Oxid. Met., 2018, 89: 251
18 Deshmukh P R, Sohn Y, Shin W G. Electrochemical performance of facile developed aqueous asymmetric (Fe,Cr)2O3//MnO2 supercapacitor[J]. Electrochim. Acta, 2018, 285: 381
19 Cheng X W, Jiang Z Y, Wei D B, et al. Characteristics of oxide scale formed on ferritic stainless steels in simulated reheating atmosphere[J]. Surf. Coat. Technol., 2014, 258: 257
20 Ellingham H J T. Reducibility of oxides and sulphides in metallurgical processes[J]. J. Soc. Chem. Ind., 1944, 63: 125
21 Jin X J, Chen S H, Rong L J. Effects of Mn on the mechanical properties and high temperature oxidation of 9Cr2WVTa steel[J]. J. Nucl. Mater., 2017, 494: 103
22 Saeki I, Konno H, Furuichi R, et al. The effect of the oxidation atmosphere on the initial oxidation of type 430 stainless steel at 1273 K[J]. Corros. Sci., 1998, 40: 191
23 Bowen A W, Leak G M. Diffusion in bcc iron base alloys[J]. Metall. Trans., 1970, 1: 2767
24 Kirkaldy J S, Smith P N, Sharma R C. Diffusion of manganese in paramagnetic BCC iron[J]. Metall. Mater. Trans., 1973, 4: 624
25 Lobnig R E, Schmidt H P, Hennesen K, et al. Diffusion of cations in chromia layers grown on iron-base alloys[J]. Oxid. Met., 1992, 37: 81
26 Lambrinou K, Koch V, Coen G, et al. Corrosion scales on various steels after exposure to liquid lead-bismuth eutectic[J]. J. Nucl. Mater., 2014, 450: 244
27 Shi Q Q, Liu J, Luan H, et al. Oxidation behavior of ferritic/martensitic steels in stagnant liquid LBE saturated by oxygen at 600oC[J]. J. Nucl. Mater., 2015, 457: 135
28 Martinelli L, Balbaud-Célérier F, Terlain A, et al. Oxidation mechanism of a Fe-9Cr-1Mo steel by liquid Pb-Bi eutectic alloy (Part I)[J]. Corros. Sci., 2008, 50: 2523
29 Martinelli L, Balbaud-Célérier F, Terlain A, et al. Oxidation mechanism of an Fe-9Cr-1Mo steel by liquid Pb-Bi eutectic alloy at 470oC (Part II)[J]. Corros. Sci., 2008, 50: 2537
30 Martinelli L, Balbaud-Célérier F, Picard G, et al. Oxidation mechanism of a Fe-9Cr-1Mo steel by liquid Pb-Bi eutectic alloy (Part III)[J]. Corros. Sci., 2008, 50: 2549
31 Xiao J, Gong X, Xiang C Y, et al. A refined oxidation mechanism proposed for ferritic-martensitic steels exposed to oxygen-saturated liquid lead-bismuth eutectic at 400oC for 500 h[J]. J. Nucl. Mater., 2021, 549: 152852
32 Huang J H. Diffusion in Metals and Alloys[M]. Beijing: Metallurgical Industry Press, 1996: 27
  黄继华. 金属及合金中的扩散[M]. 北京: 冶金工业出版社, 1996: 27
33 Parakh A, Vaidya M, Kumar N, et al. Effect of crystal structure and grain size on corrosion properties of AlCoCrFeNi high entropy alloy[J]. J. Alloys Compd., 2021, 863: 158056
34 Yu Z, Lu J T, Chen M H, et al. Effect of pre-oxidation on hot corrosion resistance of HR3C stainless steel in sulfate salt with or without Fe2O3 [J]. Corros. Sci., 2021, 192: 109789
35 F?hl H. Ionic crystals[EB/OL]. http://www.tf.uni-kiel.de/matwis/amat/def_en/kap_2/basics/b2_1_6.html
36 International Atomic Energy Agency. Comparative assessment of thermophysical and thermohydraulic characteristics of lead, lead-bismuth and sodium coolants for fast reactors[R]. Vienna: IAEA, 2002: 24
Outlines

/