Research Progress of the Surface Modification of Titanium and Titanium Alloys for Biomedical Application
Received date: 2022-03-30
Revised date: 2022-05-09
Online published: 2022-05-16
Supported by
National Natural Science Foundation of China(51771131);National Natural Science Foundation of China(52173182)
Titanium and titanium alloys have widely been used in biomedical applications as main substitutes for hard human tissues. To better meet the needs of safety, comfort, and durability of titanium and titanium alloys after implantation in the human body, the surface modification treatment of titanium and titanium alloys has become a research hotspot. In this review, based on the basic properties and existing problems of titanium and titanium alloys, the methods of surface modification for titanium and titanium alloys are introduced to improve their mechanical properties, biocompatibility, and bacteriostatic/antibacterial properties. Furthermore, the current challenges and prospects have been presented in this paper.
Zhenduo CUI , Jiamin ZHU , Hui JIANG , Shuilin WU , Shengli ZHU . Research Progress of the Surface Modification of Titanium and Titanium Alloys for Biomedical Application[J]. Acta Metall Sin, 2022 , 58(7) : 837 -856 . DOI: 10.11900/0412.1961.2022.00150
| 1 | Geetha M, Singh A K, Asokamani R, et al. Ti based biomaterials, the ultimate choice for orthopaedic implants—A review [J]. Prog. Mater. Sci., 2009, 54: 397 |
| 2 | Long M, Rack H J. Titanium alloys in total joint replacement—A materials science perspective [J]. Biomaterials, 1998, 19: 1621 |
| 3 | Elias C N, Lima J H C, Valiev R, et al. Biomedical applications of titanium and its alloys [J]. JOM, 2008, 60(3): 46 |
| 4 | Fonseca-García A, Pérez-Alvarez J, Barrera C C, et al. The effect of simulated inflammatory conditions on the surface properties of titanium and stainless steel and their importance as biomaterials [J]. Mater. Sci. Eng., 2016, C66: 119 |
| 5 | Barceloux D G. Chromium [J]. J. Toxicol.: Clin. Toxicol., 1999, 37: 173 |
| 6 | Nickens K P, Patierno S R, Ceryak S. Chromium genotoxicity: A double-edged sword [J]. Chem. Biol. Interact., 2010, 188: 276 |
| 7 | Paustenbach D J, Tvermoes B E, Unice K M, et al. A review of the health hazards posed by cobalt [J]. Crit. Rev. Toxicol., 2013, 43: 316 |
| 8 | Pavesi T, Moreira J C. Mechanisms and individuality in chromium toxicity in humans [J]. J. Appl. Toxicol., 2020, 40: 1183 |
| 9 | Kaur M, Singh K. Review on titanium and titanium based alloys as biomaterials for orthopaedic applications [J]. Mater. Sci. Eng., 2019, C102: 844 |
| 10 | Chen L Y, Cui Y W, Zhang L C. Recent development in beta titanium alloys for biomedical applications [J]. Metals, 2020, 10: 1139 |
| 11 | Niinomi M, Liu Y, Nakai M, et al. Biomedical titanium alloys with Young's moduli close to that of cortical bone [J]. Regen. Biomater., 2016, 3: 173 |
| 12 | Wang L Q, Lu W J, Qin J N, et al. Effect of precipitation phase on microstructure and superelasticity of cold-rolled beta titanium alloy during heat treatment [J]. Mater. Des., 2009, 30: 3873 |
| 13 | Wang L Q, Xie L C, Lv Y T, et al. Microstructure evolution and superelastic behavior in Ti-35Nb-2Ta-3Zr alloy processed by friction stir processing [J]. Acta Mater., 2017, 131: 499 |
| 14 | Gode C, Attarilar S, Eghbali B, et al. Electrochemical behavior of equal channel angular pressed titanium for biomedical application [C]. AIP Conf. Proc., 2015, 1653: 020041 |
| 15 | Apaza-Bedoya K, Tarce M, Benfatti C A M, et al. Synergistic interactions between corrosion and wear at titanium-based dental implant connections: A scoping review [J]. J. Periodontal Res., 2017, 52: 946 |
| 16 | Goldberg J R, Gilbert J L, Jacobs J J, et al. A multicenter retrieval study of the taper interfaces of modular hip prostheses [J]. Clin. Orthop. Relat. Res., 2002, 401: 149 |
| 17 | Takai S, Yoshino N, Kusaka Y, et al. Dissemination of metals from a failed patellar component made of titanium-base alloy [J]. J. Arthroplasty, 2003, 18: 931 |
| 18 | Moretti B, Pesce V, Maccagnano G, et al. Peripheral neuropathy after hip replacement failure: Is vanadium the culprit? [J]. Lancet, 2012, 379: 1676 |
| 19 | Gilbert J L, Mali S, Urban R M, et al. In vivo oxide-induced stress corrosion cracking of Ti-6Al-4V in a neck-stem modular taper: Emergent behavior in a new mechanism of in vivo corrosion [J]. J. Biomed. Mater. Res., 2012, 100B: 584 |
| 20 | Tsaryk R, Peters K, Barth S, et al. The role of oxidative stress in pro-inflammatory activation of human endothelial cells on Ti6Al4V alloy [J]. Biomaterials, 2013, 34: 8075 |
| 21 | Mouthuy P A, Snelling S J B, Dakin S G, et al. Biocompatibility of implantable materials: An oxidative stress viewpoint [J]. Biomaterials, 2016, 109: 55 |
| 22 | Kasai Y, Iida R, Uchida A. Metal concentrations in the serum and hair of patients with titanium alloy spinal implants [J]. Spine, 2003, 28: 1320 |
| 23 | Verstraeten S V, Aimo L, Oteiza P I. Aluminium and lead: Molecular mechanisms of brain toxicity [J]. Arch. Toxicol., 2008, 82: 789 |
| 24 | Jafari M S, Coyle C, Mortazavi J S M, et al. Revision hip arthroplasty: Infection is the most common cause of failure [J]. Clin. Orthop. Relat. Res., 2010, 468: 2046 |
| 25 | Le D H, Goodman S B, Maloney W J, et al. Current modes of failure in TKA: Infection, instability, and stiffness predominate [J]. Clin. Orthop. Relat. Res., 2014, 472: 2197 |
| 26 | Chouirfa H, Bouloussa H, Migonney V, et al. Review of titanium surface modification techniques and coatings for antibacterial applications [J]. Acta Biomater., 2019, 83: 37 |
| 27 | Maher S, Mazinani A, Barati M R, et al. Engineered titanium implants for localized drug delivery: Recent advances and perspectives of titania nanotubes arrays [J]. Expert Opin. Drug Deliv., 2018, 15: 1021 |
| 28 | Correa D R N, Kuroda P A B, Lourenço M L, et al. Development of Ti-15Zr-Mo alloys for applying as implantable biomedical devices [J]. J. Alloys Compd., 2018, 749: 163 |
| 29 | Bai Y J, Deng Y, Zheng Y F, et al. Characterization, corrosion behavior, cellular response and in vivo bone tissue compatibility of titanium-niobium alloy with low Young's modulus [J]. Mater. Sci. Eng., 2016, C59: 565 |
| 30 | Ou K L, Weng C C, Lin Y H, et al. A promising of alloying modified beta-type titanium-niobium implant for biomedical applications: Microstructural characteristics, in vitro biocompatibility and antibacterial performance [J]. J. Alloys Compd., 2017, 697: 231 |
| 31 | Zhou Y, Li Y X, Yang X J, et al. Influence of Zr content on phase transformation, microstructure and mechanical properties of Ti75 - x Nb25Zr x (x = 0-6) alloys [J]. J. Alloys Compd., 2009, 486: 628 |
| 32 | Qiu K J, Liu Y, Zhou F Y, et al. Microstructure, mechanical properties, castability and in vitro biocompatibility of Ti-Bi alloys developed for dental applications [J]. Acta Biomater., 2015, 15: 254 |
| 33 | Ahn H, Lee D, Lee K M, et al. Oxidation behavior and corrosion resistance of Ti-10Ta-10Nb alloy [J]. Surf. Coat. Technol., 2008, 202: 5784 |
| 34 | Nune K C, Misra R D K, Li S J, et al. Osteoblast cellular activity on low elastic modulus Ti-24Nb-4Zr-8Sn alloy [J]. Dent. Mater., 2017, 33: 152 |
| 35 | Zheng Y F, Zhang B B, Wang B L, et al. Introduction of antibacterial function into biomedical TiNi shape memory alloy by the addition of element Ag [J]. Acta Biomater., 2011, 7: 2758 |
| 36 | Li H B, Cui Z D, Li Z Y, et al. Effect of gas nitriding treatment on cavitation erosion behavior of commercially pure Ti and Ti-6Al-4V alloy [J]. Surf. Coat. Technol., 2013, 221: 29 |
| 37 | Li H B, Cui Z D, Li Z Y, et al. Microstructure and cavitation erosion properties of ceramic coatings fabricated on Ti-6Al-4V alloy by pack carburizing [J]. J. Mater. Eng. Perform., 2014, 23: 2772 |
| 38 | Zhu Y H, Wang W, Jia X Y, et al. Deposition of TiC film on titanium for abrasion resistant implant material by ion-enhanced triode plasma CVD [J]. Appl. Surf. Sci., 2012, 262: 156 |
| 39 | Li Q, Niinomi M, Nakai M, et al. Improvements in the superelasticity and change in deformation mode of β-type TiNb24Zr2 alloys caused by aging treatments [J]. Metall. Mater. Trans., 2011, 42A: 2843 |
| 40 | Liu Y, Li K Y, Luo T, et al. Powder metallurgical low-modulus Ti-Mg alloys for biomedical applications [J]. Mater. Sci. Eng., 2015, C56: 241 |
| 41 | Karre R, Kodli B K, Rajendran A, et al. Comparative study on Ti-Nb binary alloys fabricated through spark plasma sintering and conventional P/M routes for biomedical application [J]. Mater. Sci. Eng., 2019, C94: 619 |
| 42 | Attar H, Calin M, Zhang L C, et al. Manufacture by selective laser melting and mechanical behavior of commercially pure titanium [J]. Mater. Sci. Eng., 2014, A593: 170 |
| 43 | Li X P, Van Humbeeck J, Kruth J P. Selective laser melting of weak-textured commercially pure titanium with high strength and ductility: A study from laser power perspective [J]. Mater. Des., 2017, 116: 352 |
| 44 | García I, De Damborenea J J. Corrosion properties of tin prepared by laser gas alloying of Ti and Ti6Al4V [J]. Corros. Sci., 1998, 40: 1411 |
| 45 | Jiang P, He X L, Li X X, et al. Wear resistance of a laser surface alloyed Ti-6Al-4V alloy [J]. Surf. Coat. Technol., 2000, 130: 24 |
| 46 | Yue T M, Yu J K, Mei Z, et al. Excimer laser surface treatment of Ti-6Al-4V alloy for corrosion resistance enhancement [J]. Mater. Lett., 2002, 52: 206 |
| 47 | Hays S J. Therapeutic approaches to the treatment of neuroinflammatory diseases [J]. Curr. Pharm. Des., 1998, 4: 335 |
| 48 | Wang D, He G, Tian Y, et al. Dual effects of acid etching on cell responses and mechanical properties of porous titanium with controllable open-porous structure [J]. J. Biomed. Mater. Res., 2020, 108B: 2386 |
| 49 | Szmukler-Moncler S, Perrin D, Ahossi V, et al. Biological properties of acid etched titanium implants: Effect of sandblasting on bone anchorage [J]. J. Biomed. Mater. Res., 2004, 68B: 149 |
| 50 | Baleani M, Viceconti M, Toni A. The effect of sandblasting treatment on endurance properties of titanium alloy hip prostheses [J]. Artif. Organs, 2000, 24: 296 |
| 51 | Szmukler-Moncler S, Testori T, Bernard J P. Etched implants: A comparative surface analysis of four implant systems [J]. J. Biomed. Mater. Res., 2004, 69B: 46 |
| 52 | Wennerberg A, Albrektsson T. Effects of titanium surface topography on bone integration: A systematic review [J]. Clin. Oral Implants Res., 2009, 20: 172 |
| 53 | Klokkevold P R, Johnson P, Dadgostari S, et al. Early endosseous integration enhanced by dual acid etching of titanium: A torque removal study in the rabbit [J]. Clin. Oral Implants Res., 2001, 12: 350 |
| 54 | Ferraris S, Venturello A, Miola M, et al. Antibacterial and bioactive nanostructured titanium surfaces for bone integration [J]. Appl. Surf. Sci., 2014, 311: 279 |
| 55 | Li J, Zhou P, Attarilar S, et al. Innovative surface modification procedures to achieve micro/nano-graded Ti-based biomedical alloys and implants [J]. Coatings, 2021, 11: 647 |
| 56 | Chiang H J, Hsu H J, Peng P W, et al. Early bone response to machined, sandblasting acid etching (SLA) and novel surface-functionalization (SLAffinity) titanium implants: Characterization, biomechanical analysis and histological evaluation in pigs [J]. J. Biomed. Mater. Res., 2016, 104A: 397 |
| 57 | Gupta N, Santhiya D, Murugavel S, et al. Effects of transition metal ion dopants (Ag, Cu and Fe) on the structural, mechanical and antibacterial properties of bioactive glass [J]. Colloids Surf., 2018, 538A: 393 |
| 58 | Attarilar S, Ebrahimi M, Djavanroodi F, et al. 3D printing technologies in metallic implants: A thematic review on the techniques and procedures [J]. Int. J. Bioprint., 2021, 7: 306 |
| 59 | Kurella A, Dahotre N B. Review paper: Surface modification for bioimplants: The role of laser surface engineering [J]. J. Biomater. Appl., 2005, 20: 5 |
| 60 | Tiainen L, Abreu P, Buciumeanu M, et al. Novel laser surface texturing for improved primary stability of titanium implants [J]. J. Mech. Behav. Biomed. Mater., 2019, 98: 26 |
| 61 | Cunha A, Elie A M, Plawinski L, et al. Femtosecond laser surface texturing of titanium as a method to reduce the adhesion of Staphylococcus aureus and biofilm formation [J]. Appl. Surf. Sci., 2016, 360: 485 |
| 62 | Lee B H, Kim J K, Kim Y D, et al. In vivo behavior and mechanical stability of surface-modified titanium implants by plasma spray coating and chemical treatments [J]. J. Biomed. Mater. Res., 2004, 69A: 279 |
| 63 | Sargin F, Erdogan G, Kanbur K, et al. Investigation of in vitro behavior of plasma sprayed Ti, TiO2 and HA coatings on peek [J]. Surf. Coat. Technol., 2021, 411: 126965 |
| 64 | Khor K A, Gu Y W, Quek C H, et al. Plasma spraying of functionally graded hydroxyapatite/Ti-6Al-4V coatings [J]. Surf. Coat. Technol., 2003, 168: 195 |
| 65 | Hameed P, Gopal V, Bjorklund S, et al. Axial suspension plasma spraying: An ultimate technique to tailor Ti6Al4V surface with hap for orthopaedic applications [J]. Colloids Surf., 2019, 173B: 806 |
| 66 | Singh H, Prakash C, Singh S. Plasma spray deposition of HA-TiO2 on β-phase Ti-35Nb-7Ta-5Zr alloy for hip stem: Characterization of bio-mechanical properties, wettability, and wear resistance [J]. J. Bionic Eng., 2020, 17: 1029 |
| 67 | Duta L. In vivo assessment of synthetic and biological-derived calcium phosphate-based coatings fabricated by pulsed laser deposition: A review [J]. Coatings, 2021, 11: 99 |
| 68 | Galindo-Valdés J S, Cortés-Hernández D A, Ortiz-Cuellar J C, et al. Laser deposition of bioactive coatings by in situ synthesis of pseudowollastonite on Ti6Al4V alloy [J]. Opt. Laser Technol., 2021, 134: 106586 |
| 69 | Cao J X, Lian R Z, Jiang X H. Magnesium and fluoride doped hydroxyapatite coatings grown by pulsed laser deposition for promoting titanium implant cytocompatibility [J]. Appl. Surf. Sci., 2020, 515: 146069 |
| 70 | Zaveri N, Mahapatra M, Deceuster A, et al. Corrosion resistance of pulsed laser-treated Ti-6Al-4V implant in simulated biofluids [J]. Electrochim. Acta, 2008, 53: 5022 |
| 71 | Chen L Y, Komasa S, Hashimoto Y, et al. In vitro and in vivo osteogenic activity of titanium implants coated by pulsed laser deposition with a thin film of fluoridated hydroxyapatite [J]. Int. J. Mol. Sci., 2018, 19: 1127 |
| 72 | Pelletier H, Nelea V, Mille P, et al. Mechanical properties of pulsed laser-deposited hydroxyapatite thin film implanted at high energy with N+ and Ar+ ions. Part I: nanoindentation with spherical tipped indenter [J]. Nucl. Instrum. Methods Phys. Res., 2004, 216B: 269 |
| 73 | D'Alessio L, Ferro D, Marotta V, et al. Laser ablation and deposition of bioglass® 45S5 thin films [J]. Appl. Surf. Sci., 2001, 183: 10 |
| 74 | Gnanavel S, Ponnusamy S, Mohan L, et al. Electrochemical behavior of biomedical titanium alloys coated with diamond carbon in Hanks' solution [J]. J. Mater. Eng. Perform., 2018, 27: 1635 |
| 75 | Kaliaraj G S, Bavanilathamuthiah M, Kirubaharan K, et al. Bio-inspired YSZ coated titanium by EB-PVD for biomedical applications [J]. Surf. Coat. Technol., 2016, 307: 227 |
| 76 | Paital S R, Dahotre N B. Calcium phosphate coatings for bio-implant applications: Materials, performance factors, and methodologies [J]. Mater. Sci. Eng., 2009, R66: 1 |
| 77 | Oyane A, Wang X P, Sogo Y, et al. Calcium phosphate composite layers for surface-mediated gene transfer [J]. Acta Biomater., 2012, 8: 2034 |
| 78 | Surmenev R A, Surmeneva M A, Ivanova A A. Significance of calcium phosphate coatings for the enhancement of new bone osteogenesis—A review [J]. Acta Biomater., 2014, 10: 557 |
| 79 | Liu B, Shi X M, Xiao G Y, et al. In-situ preparation of scholzite conversion coatings on titanium and Ti-6Al-4V for biomedical applications [J]. Colloids Surf., 2017, 153B: 291 |
| 80 | Yu W Z, Zhang Y Z, Liu X M, et al. Synergistic antibacterial activity of multi components in lysozyme/chitosan/silver/hydroxyapatite hybrid coating [J]. Mater. Des., 2018, 139: 351 |
| 81 | Liu X H, Wu L, Ai H J, et al. Cytocompatibility and early osseointegration of nano TiO2-modified Ti-24Nb-4Zr-7.9Sn surfaces [J]. Mater. Sci. Eng., 2015, C48: 256 |
| 82 | Zhang X M, Li Z Y, Yuan X B, et al. Fabrication of dopamine-modified hyaluronic acid/chitosan multilayers on titanium alloy by layer-by-layer self-assembly for promoting osteoblast growth [J]. Appl. Surf. Sci., 2013, 284: 732 |
| 83 | İzmir M, Ercan B. Anodization of titanium alloys for orthopedic applications [J]. Front. Chem. Sci. Eng., 2019, 13: 28 |
| 84 | Minagar S, Berndt C C, Wang J, et al. A review of the application of anodization for the fabrication of nanotubes on metal implant surfaces [J]. Acta Biomater., 2012, 8: 2875 |
| 85 | Schwartz Z, Olivares-Navarrete R, Wieland M, et al. Mechanisms regulating increased production of osteoprotegerin by osteoblasts cultured on microstructured titanium surfaces [J]. Biomaterials, 2009, 30: 3390 |
| 86 | Kim M J, Kim C W, Lim Y J, et al. Microrough titanium surface affects biologic response in MG63 osteoblast-like cells [J]. J. Biomed. Mater. Res., 2006, 79A: 1023 |
| 87 | Yu W Q, Jiang X Q, Zhang F Q, et al. The effect of anatase TiO2 nanotube layers on MC3T3-E1 preosteoblast adhesion, proliferation, and differentiation [J]. J. Biomed. Mater. Res., 2010, 94A: 1012 |
| 88 | Zhao L Z, Mei S L, Chu P K, et al. The influence of hierarchical hybrid micro/nano-textured titanium surface with titania nanotubes on osteoblast functions [J]. Biomaterials, 2010, 31: 5072 |
| 89 | Huang X B, Liu Y P, Yu H W, et al. One-step fabrication of cytocompatible micro/nano-textured surface with TiO2 mesoporous arrays on titanium by high current anodization [J]. Electrochim. Acta, 2016, 199: 116 |
| 90 | Hu N, Wu Y Z, Xie L X, et al. Enhanced interfacial adhesion and osseointegration of anodic TiO2 nanotube arrays on ultra-fine-grained titanium and underlying mechanisms [J]. Acta Biomater., 2020, 106: 360 |
| 91 | Lee J K, Choi D S, Jang I, et al. Improved osseointegration of dental titanium implants by TiO2 nanotube arrays with recombinant human bone morphogenetic protein-2: A pilot in vivo study [J]. Int. J. Nanomedicine, 2015, 10: 1145 |
| 92 | Su E P, Justin D E, Pratt C R, et al. Effects of titanium nanotubes on the osseointegration, cell differentiation, mineralisation and antibacterial properties of orthopaedic implant surfaces [J]. Bone Joint J., 2018, 100-B: 9 |
| 93 | Kim S Y, Kim Y K, Park I S, et al. Effect of alkali and heat treatments for bioactivity of TiO2 nanotubes [J]. Appl. Surf. Sci., 2014, 321: 412 |
| 94 | Kang M K, Moon S K, Kim K M, et al. Antibacterial effect and cytocompatibility of nano-structured TiO2 film containing Cl [J]. Dent. Mater. J., 2011, 30: 790 |
| 95 | Liang Y Q, Yang X J, Cui Z D, et al. Self-organized nanotubular layer on Ti-4Zr-22Nb-2Sn alloys formed in organic electrolytes [J]. J. Mater. Res., 2009, 24: 3647 |
| 96 | Shin K R, Kim Y S, Kim G W, et al. Effects of concentration of Ag nanoparticles on surface structure and in vitro biological responses of oxide layer on pure titanium via plasma electrolytic oxidation [J]. Appl. Surf. Sci., 2015, 347: 574 |
| 97 | Kaluđerović M R, Schreckenbach J P, Graf H L. First titanium dental implants with white surfaces: Preparation and in vitro tests [J]. Dent. Mater., 2014, 30: 759 |
| 98 | Wang H Y, Zhu R F, Lu Y P, et al. Preparation and properties of plasma electrolytic oxidation coating on sandblasted pure titanium by a combination treatment [J]. Mater. Sci. Eng., 2014, C42: 657 |
| 99 | Hong M H, Lee D H, Kim K M, et al. Study on bioactivity and bonding strength between Ti alloy substrate and TiO2 film by micro-arc oxidation [J]. Thin Solid Films, 2011, 519: 7065 |
| 100 | Wang R Y, He X J, Gao Y E, et al. Antimicrobial property, cytocompatibility and corrosion resistance of Zn-doped ZrO2/TiO2 coatings on Ti6Al4V implants [J]. Mater. Sci. Eng., 2017, C75: 7 |
| 101 | Matos A O, Ricomini-Filho A P, Beline T, et al. Three-species biofilm model onto plasma-treated titanium implant surface [J]. Colloids Surf., 2017, 152B: 354 |
| 102 | Zhang J, Tu Q S, Bonewald L F, et al. Effects of miR-335-5p in modulating osteogenic differentiation by specifically downregulating Wnt antagonist DKK1 [J]. J. Bone Miner. Res., 2011, 26: 1953 |
| 103 | Li Y, Fan L K, Liu S Y, et al. The promotion of bone regeneration through positive regulation of angiogenic-osteogenic coupling using microRNA-26a [J]. Biomaterials, 2013, 34: 5048 |
| 104 | Suh J S, Lee J Y, Choi Y S, et al. Erratum to ‘Peptide-mediated intracellular delivery of miRNA-29b for osteogenic stem cell differentiation' [Biomaterials 34 (2013) 4347-4359] [J]. Biomaterials, 2014, 35: 5039 |
| 105 | Meng Y B, Li X, Li Z Y, et al. Surface functionalization of titanium alloy with miR-29b nanocapsules to enhance bone regeneration [J]. ACS Appl. Mater. Interfaces, 2016, 8: 5783 |
| 106 | Geng Z, Wang X G, Zhao J, et al. The synergistic effect of strontium-substituted hydroxyapatite and microRNA-21 on improving bone remodeling and osseointegration [J]. Biomater. Sci., 2018, 6: 2694 |
| 107 | Geng Z, Yu Y M, Li Z Y, et al. Mir-21 promotes osseointegration and mineralization through enhancing both osteogenic and osteoclastic expression [J]. Mater. Sci. Eng., 2020, C111: 110785 |
| 108 | Zhang X M, Zhu S L, Li Z Y, et al. Multilayer modification on titanium surface for in situ delivery of MicroRNAs [J]. Mater. Lett., 2014, 133: 243 |
| 109 | Shahriyari F, Razaghian A, Taghiabadi R, et al. Effect of friction hardening pre-treatment on increasing cytocompatibility of alkali heat-treated Ti-6Al-4V alloy [J]. Surf. Coat. Technol., 2018, 353: 148 |
| 110 | Sun Y S, Chang J H, Huang H H. Enhancing the biological response of titanium surface through the immobilization of bone morphogenetic protein-2 using the natural cross-linker genipin [J]. Surf. Coat. Technol., 2016, 303: 289 |
| 111 | Hu H, Cui Z D, Zhu S L, et al. Preparation of hydroxyapatite layer on Ti-based bulk metallic glasses by acid and alkali pre-treatment [J]. Rare Met., 2015, 34: 22 |
| 112 | Chen M F, Liu D B, You C, et al. Interfacial characteristic of graded hydroxyapatite and titanium thin film by magnetron sputtering [J]. Surf. Coat. Technol., 2007, 201: 5688 |
| 113 | Li M, Li L Q, Su K, et al. Highly effective and noninvasive near-infrared eradication of a Staphylococcus aureus biofilm on implants by a photoresponsive coating within 20 min [J]. Adv. Sci., 2019, 6: 1900599 |
| 114 | Tan L, Li J, Liu X M, et al. Rapid biofilm eradication on bone implants using red phosphorus and near-infrared light [J]. Adv. Mater., 2018, 30: 1801808 |
| 115 | Hosseinabadi H N, Sajjady S A, Amini S. Creating micro textured surfaces for the improvement of surface wettability through ultrasonic vibration assisted turning [J]. Int. J. Adv. Manuf. Technol., 2018, 96: 2825 |
| 116 | Gao X J, Tong W J, Ouyang X P, et al. Facile fabrication of a superhydrophobic titanium surface with mechanical durability by chemical etching [J]. RSC Adv., 2015, 5: 84666 |
| 117 | Hou X M, Wang X B, Zhu Q S, et al. Preparation of polypropylene superhydrophobic surface and its blood compatibility [J]. Colloids Surf., 2010, 80B: 247 |
| 118 | Tang P F, Zhang W, Wang Y, et al. Effect of superhydrophobic surface of titanium on Staphylococcus aureus adhesion [J]. J. Nanomater., 2011, 2011: 178921 |
| 119 | Zhang X, Wan Y, Ren B, et al. Preparation of superhydrophobic surface on titanium alloy via micro-milling, anodic oxidation and fluorination [J]. Micromachines, 2020, 11: 316 |
| 120 | Patiño-Herrera R, González-Alatorre G, Estrada-Baltazar A, et al. Hydrophobic coatings for prevention of dental enamel erosion [J]. Surf. Coat. Technol., 2015, 275: 148 |
| 121 | Mi G J, Shi D, Wang M, et al. Reducing bacterial infections and biofilm formation using nanoparticles and nanostructured antibacterial surfaces [J]. Adv. Healthc. Mater., 2018, 7: 1800103 |
| 122 | Kingshott P, Wei J, Bagge-Ravn D, et al. Covalent attachment of poly(ethylene glycol) to surfaces, critical for reducing bacterial adhesion [J]. Langmuir, 2003, 19: 6912 |
| 123 | Harris L G, Tosatti S, Wieland M, et al. Staphylococcus aureus adhesion to titanium oxide surfaces coated with non-functionalized and peptide-functionalized poly(l-lysine)-grafted-poly(ethylene glycol) copolymers [J]. Biomaterials, 2004, 25: 4135 |
| 124 | Yang F, Williams C G, Wang D A, et al. The effect of incorporating RGD adhesive peptide in polyethylene glycol diacrylate hydrogel on osteogenesis of bone marrow stromal cells [J]. Biomaterials, 2005, 26: 5991 |
| 125 | Ding X, Yang C, Lim T P, et al. Antibacterial and antifouling catheter coatings using surface grafted PEG-b-cationic polycarbonate diblock copolymers [J]. Biomaterials, 2012, 33: 6593 |
| 126 | Yang C, Ding X, Ono R J, et al. Brush-like polycarbonates containing dopamine, cations, and PEG providing a broad-spectrum, antibacterial, and antifouling surface via one-step coating [J]. Adv. Mater., 2014, 26: 7346 |
| 127 | Li L L, Qi G B, Yu F Q, et al. An adaptive biointerface from self-assembled functional peptides for tissue engineering [J]. Adv. Mater., 2015, 27: 3181 |
| 128 | Ivanova E P, Hasan J, Webb H K, et al. Bactericidal activity of black silicon [J]. Nat. Commun., 2013, 4: 2838 |
| 129 | Mainwaring D E, Nguyen S H, Webb H, et al. The nature of inherent bactericidal activity: Insights from the nanotopology of three species of dragonfly [J]. Nanoscale, 2016, 8: 6527 |
| 130 | Li J, Tan L, Liu X M, et al. Balancing bacteria-osteoblast competition through selective physical puncture and biofunctionalization of ZnO/polydopamine/arginine-glycine-aspartic acid-cysteine nanorods [J]. ACS Nano, 2017, 11: 11250 |
| 131 | Zhong Z X, Xu Z, Sheng T, et al. Unusual air filters with ultrahigh efficiency and antibacterial functionality enabled by ZnO nanorods [J]. ACS Appl. Mater. Interfaces, 2015, 7: 21538 |
| 132 | Nguyen M N, Lebarbe T, Zouani O F, et al. Impact of RGD nanopatterns grafted onto titanium on osteoblastic cell adhesion [J]. Biomacromolecules, 2012, 13: 896 |
| 133 | Bellis S L. Advantages of RGD peptides for directing cell association with biomaterials [J]. Biomaterials, 2011, 32: 4205 |
| 134 | Swartjes J J T M, Das T, Sharifi S, et al. A functional DNase I coating to prevent adhesion of bacteria and the formation of biofilm [J]. Adv. Funct. Mater., 2013, 23: 2843 |
| 135 | Flemming H C, Wingender J. The biofilm matrix [J]. Nat. Rev. Microbiol., 2010, 8: 623 |
| 136 | Arciola C R, Campoccia D, Montanaro L. Implant infections: Adhesion, biofilm formation and immune evasion [J]. Nat. Rev. Microbiol., 2018, 16: 397 |
| 137 | Chen Z W, Ji H W, Liu C Q, et al. A multinuclear metal complex based dnase-mimetic artificial enzyme: Matrix cleavage for combating bacterial biofilms [J]. Angew. Chem. Int. Ed., 2016, 55: 10732 |
| 138 | Liu Z W, Wang F M, Ren J S, et al. A series of MOF/Ce-based nanozymes with dual enzyme-like activity disrupting biofilms and hindering recolonization of bacteria [J]. Biomaterials, 2019, 208: 21 |
| 139 | Miller M B, Bassler B L. Quorum sensing in bacteria [J]. Annu. Rev. Microbiol., 2001, 55: 165 |
| 140 | Waters C M, Bassler B L. Quorum sensing: Cell-to-cell communication in bacteria [J]. Annu. Rev. Cell. Dev. Biol., 2005, 21: 319 |
| 141 | Flickinger S T, Copeland M F, Downes E M, et al. Quorum sensing between Pseudomonas aeruginosa biofilms accelerates cell growth [J]. J. Am. Chem. Soc., 2011, 133: 5966 |
| 142 | Sun Y H, Qin H S, Yan Z Q, et al. Combating biofilm associated infection in vivo: Integration of quorum sensing inhibition and photodynamic treatment based on multidrug delivered hollow carbon nitride sphere [J]. Adv. Funct. Mater., 2019, 29: 1808222 |
| 143 | Vermote A, Brackman G, Risseeuw M D P, et al. Hamamelitannin analogues that modulate quorum sensing as potentiators of antibiotics against Staphylococcus aureus [J]. Angew. Chem. Int. Ed., 2016, 55: 6551 |
| 144 | Ivanova K, Fernandes M M, Mendoza E, et al. Enzyme multilayer coatings inhibit Pseudomonas aeruginosa biofilm formation on urinary catheters [J]. Appl. Microbiol. Biotechnol., 2015, 99: 4373 |
| 145 | Yuan Z, He Y, Lin C C, et al. Antibacterial surface design of biomedical titanium materials for orthopedic applications [J]. J. Mater. Sci. Technol., 2021, 78: 51 |
| 146 | Handke L D, Rogers K L, Olson M E, et al. Staphylococcus epidermidis saeR is an effector of anaerobic growth and a mediator of acute inflammation [J]. Infect. Immun., 2008, 76: 141 |
| 147 | Yang S B, Han X G, Yang Y, et al. Bacteria-targeting nanoparticles with microenvironment-responsive antibiotic release to eliminate intracellular Staphylococcus aureus and associated infection [J]. ACS Appl. Mater. Interfaces, 2018, 10: 14299 |
| 148 | Chatterjee S S, Joo H S, Duong A C, et al. Essential Staphylococcus aureus toxin export system [J]. Nat. Med., 2013, 19: 364 |
| 149 | Sutrisno L, Hu Y, Shen X K, et al. Fabrication of hyaluronidase-responsive biocompatible multilayers on BMP2 loaded titanium nanotube for the bacterial infection prevention [J]. Mater. Sci. Eng., 2018, C89: 95 |
| 150 | Zhuk I, Jariwala F, Attygalle A B, et al. Self-defensive layer-by-layer films with bacteria-triggered antibiotic release [J]. ACS Nano, 2014, 8: 7733 |
| 151 | Yuan Z, Huang S Z, Lan S X, et al. Surface engineering of titanium implants with enzyme-triggered antibacterial properties and enhanced osseointegration in vivo [J]. J. Mater. Chem., 2018, 6B: 8090 |
| 152 | Jia Z J, Xiu P, Li M, et al. Bioinspired anchoring AgNPs onto micro-nanoporous TiO2 orthopedic coatings: Trap-killing of bacteria, surface-regulated osteoblast functions and host responses [J]. Biomaterials, 2016, 75: 203 |
| 153 | Lin X, Yang S F, Lai K, et al. Orthopedic implant biomaterials with both osteogenic and anti-infection capacities and associated in vivo evaluation methods [J]. Nanomed: Nanotechnol. Biol. Med., 2017, 13: 123 |
| 154 | Afewerki S, Bassous N, Harb S, et al. Advances in dual functional antimicrobial and osteoinductive biomaterials for orthopaedic applications [J]. Nanomed: Nanotechnol., Biol. Med., 2020, 24: 102143 |
| 155 | Wang Z M, Wang K F, Lu X, et al. Nanostructured architectures by assembling polysaccharide-coated BSA nanoparticles for biomedical application [J]. Adv. Healthc. Mater., 2015, 4: 927 |
| 156 | Min J, Choi K Y, Dreaden E C, et al. Designer dual therapy nanolayered implant coatings eradicate biofilms and accelerate bone tissue repair [J]. ACS Nano, 2016, 10: 4441 |
| 157 | Verlee A, Mincke S, Stevens C V. Recent developments in antibacterial and antifungal chitosan and its derivatives [J]. Carbohydr. Polym., 2017, 164: 268 |
| 158 | Chua P H, Neoh K G, Kang E T, et al. Surface functionalization of titanium with hyaluronic acid/chitosan polyelectrolyte multilayers and RGD for promoting osteoblast functions and inhibiting bacterial adhesion [J]. Biomaterials, 2008, 29: 1412 |
| 159 | Ordikhani F, Tamjid E, Simchi A. Characterization and antibacterial performance of electrodeposited chitosan-vancomycin composite coatings for prevention of implant-associated infections [J]. Mater. Sci. Eng., 2014, C41: 240 |
| 160 | Lin J, Qiu S Y, Lewis K, et al. Mechanism of bactericidal and fungicidal activities of textiles covalently modified with alkylated polyethylenimine [J]. Biotechnol. Bioeng., 2003, 83: 168 |
| 161 | Atar-Froyman L, Sharon A, Weiss E I, et al. Anti-biofilm properties of wound dressing incorporating nonrelease polycationic antimicrobials [J]. Biomaterials, 2015, 46: 141 |
| 162 | Asri L A T W, Crismaru M, Roest S, et al. A shape-adaptive, antibacterial-coating of immobilized quaternary-ammonium compounds tethered on hyperbranched polyurea and its mechanism of action [J]. Adv. Funct. Mater., 2014, 24: 346 |
| 163 | Wei T, Zhan W J, Yu Q, et al. Smart biointerface with photoswitched functions between bactericidal activity and bacteria-releasing ability [J]. ACS Appl. Mater. Interfaces, 2017, 9: 25767 |
| 164 | Zasloff M. Antimicrobial peptides of multicellular organisms [J]. Nature, 2002, 415: 389 |
| 165 | Reddy K V R, Yedery R D, Aranha C. Antimicrobial peptides: Premises and promises [J]. Int. J. Antimicrob. Agents, 2004, 24: 536 |
| 166 | Brogden K A. Antimicrobial peptides: Pore formers or metabolic inhibitors in bacteria? [J]. Nat. Rev. Microbiol., 2005, 3: 238 |
| 167 | Campoccia D, Montanaro L, Arciola C R. A review of the biomaterials technologies for infection-resistant surfaces [J]. Biomaterials, 2013, 34: 8533 |
| 168 | Mellier C, Fayon F, Boukhechba F, et al. Design and properties of novel gallium-doped injectable apatitic cements [J]. Acta Biomater., 2015, 24: 322 |
| 169 | Mei S L, Wang H Y, Wang W, et al. Antibacterial effects and biocompatibility of titanium surfaces with graded silver incorporation in titania nanotubes [J]. Biomaterials, 2014, 35: 4255 |
| 170 | Zhang L, Gao Q, Han Y. Zn and Ag co-doped anti-microbial TiO2 coatings on Ti by micro-arc oxidation [J]. J. Mater. Sci. Technol., 2016, 32: 919 |
| 171 | Sedelnikova M B, Komarova E G, Sharkeev Y P, et al. Modification of titanium surface via Ag-, Sr- and Si-containing micro-arc calcium phosphate coating [J]. Bioact. Mater., 2019, 4: 224 |
| 172 | Roknian M, Fattah-alhosseini A, Gashti S O, et al. Study of the effect of ZnO nanoparticles addition to PEO coatings on pure titanium substrate: Microstructural analysis, antibacterial effect and corrosion behavior of coatings in ringer's physiological solution [J]. J. Alloys Compd., 2018, 740: 330 |
| 173 | Liu W W, Su P L, Chen S, et al. Synthesis of TiO2 nanotubes with ZnO nanoparticles to achieve antibacterial properties and stem cell compatibility [J]. Nanoscale, 2014, 6: 9050 |
| 174 | Maimaiti B, Zhang N Y, Yan L, et al. Stable ZnO-doped hydroxyapatite nanocoating for anti-infection and osteogenic on titanium [J]. Colloids Surf., 2020, 186B: 110731 |
| 175 | Ma Z, Ren L, Shahzad M B, et al. Hot deformation behavior of Cu-bearing antibacterial titanium alloy [J]. J. Mater. Sci. Technol., 2018, 34: 1867 |
| 176 | Liu H, Liu R, Ullah I, et al. Rough surface of copper-bearing titanium alloy with multifunctions of osteogenic ability and antibacterial activity [J]. J. Mater. Sci. Technol., 2020, 48: 130 |
| 177 | Liu R, Tang Y L, Liu H, et al. Effects of combined chemical design (Cu addition) and topographical modification (SLA) of Ti-Cu/SLA for promoting osteogenic, angiogenic and antibacterial activities [J]. J. Mater. Sci. Technol., 2020, 47: 202 |
| 178 | Agarwal A, Weis T L, Schurr M J, et al. Surfaces modified with nanometer-thick silver-impregnated polymeric films that kill bacteria but support growth of mammalian cells [J]. Biomaterials, 2010, 31: 680 |
| 179 | Cheng H, Xiong W, Fang Z, et al. Strontium (Sr) and silver (Ag) loaded nanotubular structures with combined osteoinductive and antimicrobial activities [J]. Acta Biomater., 2016, 31: 388 |
| 180 | Tîlmaciu C M, Mathieu M, Lavigne J P, et al. In vitro and in vivo characterization of antibacterial activity and biocompatibility: A study on silver-containing phosphonate monolayers on titanium [J]. Acta Biomater., 2015, 15: 266 |
| 181 | van Hengel I A J, Putra N E, Tierolf M W A M, et al. Biofunctionalization of selective laser melted porous titanium using silver and zinc nanoparticles to prevent infections by antibiotic-resistant bacteria [J]. Acta Biomater., 2020, 107: 325 |
| 182 | Shen X K, Hu Y, Xu G Q, et al. Regulation of the biological functions of osteoblasts and bone formation by Zn-incorporated coating on microrough titanium [J]. ACS Appl. Mater. Interfaces, 2014, 6: 16426 |
| 183 | Jin G D, Cao H L, Qiao Y Q, et al. Osteogenic activity and antibacterial effect of zinc ion implanted titanium [J]. Colloids Surf., 2014, 117B: 158 |
| 184 | Huo K F, Zhang X M, Wang H R, et al. Osteogenic activity and antibacterial effects on titanium surfaces modified with Zn-incorporated nanotube arrays [J]. Biomaterials, 2013, 34: 3467 |
| 185 | Liu P, Zhao Y C, Yuan Z, et al. Construction of Zn-incorporated multilayer films to promote osteoblasts growth and reduce bacterial adhesion [J]. Mater. Sci. Eng., 2017, C75: 998 |
| 186 | Wu M C, Deokar A R, Liao J H, et al. Graphene-based photothermal agent for rapid and effective killing of bacteria [J]. ACS Nano, 2013, 7: 1281 |
| 187 | Wang C, Wang Y L, Zhang L L, et al. Pretreated macrophage-membrane-coated gold nanocages for precise drug delivery for treatment of bacterial infections [J]. Adv. Mater., 2018, 30: 1804023 |
| 188 | Qiao Y, Ping Y, Zhang H B, et al. Laser-activatable CuS nanodots to treat multidrug-resistant bacteria and release copper ion to accelerate healing of infected chronic nonhealing wounds [J]. ACS Appl. Mater. Interfaces, 2019, 11: 3809 |
| 189 | Yin W Y, Yu J, Lv F T, et al. Functionalized nano-MoS2 with peroxidase catalytic and near-infrared photothermal activities for safe and synergetic wound antibacterial applications [J]. ACS Nano, 2016, 10: 11000 |
| 190 | Cheng W, Zeng X W, Chen H Z, et al. Versatile polydopamine platforms: Synthesis and promising applications for surface modification and advanced nanomedicine [J]. ACS Nano, 2019, 13: 8537 |
| 191 | Lei W X, Ren K F, Chen T T, et al. Polydopamine nanocoating for effective photothermal killing of bacteria and fungus upon near-infrared irradiation [J]. Adv. Mater. Interfaces, 2016, 3: 1600767 |
| 192 | Yuan Z, Tao B L, He Y, et al. Biocompatible MoS2/PDA-RGD coating on titanium implant with antibacterial property via intrinsic ROS-independent oxidative stress and NIR irradiation [J]. Biomaterials, 2019, 217: 119290 |
| 193 | Xie X Z, Mao C Y, Liu X M, et al. Synergistic bacteria killing through photodynamic and physical actions of graphene oxide/Ag/collagen coating [J]. ACS Appl. Mater. Interfaces, 2017, 9: 26417 |
| 194 | Wang D, Niu L J, Qiao Z Y, et al. Synthesis of self-assembled porphyrin nanoparticle photosensitizers [J]. ACS Nano, 2018, 12: 3796 |
| 195 | Zhu Y W, Xu C, Zhang N, et al. Polycationic synergistic antibacterial agents with multiple functional components for efficient anti-infective therapy [J]. Adv. Funct. Mater., 2018, 28: 1706709 |
| 196 | Deng Q Q, Sun P P, Zhang L, et al. Porphyrin MOF dots-based, function-adaptive nanoplatform for enhanced penetration and photodynamic eradication of bacterial biofilms [J]. Adv. Funct. Mater., 2019, 29: 1903018 |
| 197 | Su K, Tan L, Liu X M, et al. Rapid photo-sonotherapy for clinical treatment of bacterial infected bone implants by creating oxygen deficiency using sulfur doping [J]. ACS Nano, 2020, 14: 2077 |
| 198 | Feng Z Z, Liu X M, Tan L, et al. Electrophoretic deposited stable chitosan@MoS2 coating with rapid in situ bacteria-killing ability under dual-light irradiation [J]. Small, 2018, 14: 1704347 |
| 199 | Yuan Z, Tao B L, He Y, et al. Remote eradication of biofilm on titanium implant via near-infrared light triggered photothermal/photodynamic therapy strategy [J]. Biomaterials, 2019, 223: 119479 |
/
| 〈 |
|
〉 |