Orginal Article

Study on Heating Schedule of 1000 MPa Grade Nb-Ti Microalloyed Ultra-High Strength Steel

  • Yajun HUI ,
  • Hui PAN ,
  • Wenyuan LI ,
  • Kun LIU ,
  • Bin CHEN ,
  • Yang CUI
Expand
  • 1 Sheet Metal Research Institute, Shougang Research Institute of Technology, Beijing 100043, China
    2 Beijing Key Laboratory of Green Recyclable Process for Iron & Steel Production, Shougang Group, Beijing 100043, China;

Received date: 2016-06-15

  Online published: 2016-12-13

Abstract

In the production process of ultra-high strength steel, heating schedule of casting slab is one of primary controlling parameters in hot rolling techniques. Heating temperature and holding time affect the prior austenite grain size and the solution of microalloyed elements directly, which both affect austenite recrystallization, precipitation and mechanical properties. A plenty of researches have been made to get better understanding and controlling the austenite grain size or precipitation behavior during austenitizing process over the past half a century, but it lacks systematic researches. Hence it is very important to confirm a reasonable heating schedule. In this work, the austenite grain coarsening behavior and microalloying carbonitrides dissolving behavior in 1000 MPa grade Nb-Ti microalloyed ultra-high strength steel during isothermal holding at different temperatures were studied by OM, TEM and EDS. The results showed that the precipitates in the slab can be obviously classified into three kinds by their size and shape. The average dimension of the bigger cubic precipitates is over 1 μm, and that of the smaller spherical, ellipsoid or cubic precipitates is below 500 nm or less. EDS results showed that the bigger cubic precipitates are TiN, and the smaller spherical, ellipsoid or cubic precipitates are mainly composed of Nb, Ti composite precipitates and a bit of TiS or Ti (C, S). With the increasing of holding temperature, increase of the original austenite grain size showed a monotonous increase trend, and the austenite grain grows rapidly when the heating temperature exceeds 1200 ℃; the amount of precipitates decreased and their size increased, the atomic ratio of Ti/Nb increased gradually, and EDS results showed all the precipitates contain Nb, Ti elements. With the increasing of holding time, the average austenite grain grew up in parabolic law, the amount of small sized spherical and ellipsoid precipitates dissolved gradually, and that of the large sized cubic precipitates increased gradually and their edges become blurred. The effects of heating temperature and holding time on austenite grain size and precipitation behavior were considered synthetically, the heating temperature at 1250 ℃ by holding 80 min will be more appropriate for the 1000 MPa grade Nb, Ti microalloyed ultra-high strength steel.

Cite this article

Yajun HUI , Hui PAN , Wenyuan LI , Kun LIU , Bin CHEN , Yang CUI . Study on Heating Schedule of 1000 MPa Grade Nb-Ti Microalloyed Ultra-High Strength Steel[J]. Acta Metall Sin, 2017 , 53(2) : 129 -139 . DOI: 10.11900/0412.1961.2016.00237

References

[1] Zhang P C, Wu H B, Tang D, et al.Dissolving behaviors of carbonitrides in Nb-V-Ti and V-Ti microalloying steels[J]. Acta Metall. Sin., 2007, 43: 753
[1] (张鹏程, 武会宾, 唐荻等. Nb-V-Ti和V-Ti微合金钢中碳氮化物的回溶行为[J]. 金属学报, 2007, 43: 753)
[2] Giumelli A K, Militzer M, Hawbolt E B.Analysis of the austenite grain size distribution in plain carbon steels[J]. ISIJ Int., 1999, 39: 271
[3] Papworth A J, Williams D B.Segregation to prior austenite grain boundaries in low-alloy steels[J]. Scr. Mater., 2000, 42: 1107
[4] Uhm S, Moon J, Lee C, et al.Prediction model for the austenite grain size in the coarse grained heat affected zone of Fe-C-Mn steels: Considering the effect of initial grain size on isothermal growth behavior[J]. ISIJ Int., 2004, 44: 1230
[5] Speer J G, Michael J R, Hansen S S.Carbonitride precipitation in niobium/vanadium microalloyed steels[J]. Metall. Mater. Trans., 1987, 18A: 211
[6] Yong Q L, Li Y F, Sun Z B, et al.Second-phase on grain coarsening time and temperature[J]. Iron Steel, 1993, 28(9): 45
[6] (雍岐龙, 李永福, 孙珍宝等. 第二相与晶粒粗化时间及粗化温度[J]. 钢铁, 1993, 28(9): 45)
[7] Smith R M, Dunne D P.Structural aspects of alloy carbonitride precipitation in microalloyed steels[J]. Mater. Forum, 1988, 11: 166
[8] Hong S G, Kang K B, Park C G.Strain-induced precipitation of NbC in Nb and Nb-Ti microalloyed HSLA steels[J]. Scr. Mater., 2002, 46: 163
[9] Yi H L, Du L X, Wang G D, et al.New Ti-bearing high strength steel[J]. J. Mech. Eng., 2008, 44(8): 50
[10] Dutta B, Valdes E, Sellars C M.Mechanism and kinetics of strain induced precipitation of Nb(C, N) in austenite[J]. Acta Metall. Mater., 1992, 40: 653
[11] Senuma T, Suehiro M, Yada H.Mathematical models for predicting microstructural evolution and mechanical properties of hot strips[J]. ISIJ Int., 1992, 32: 423
[12] Jiao S, Penning J, Leysen F, et al.The modeling of the grain growth in a continuous reheating process of a low carbon Si-Mn bearing TRIP steel[J]. ISIJ Int., 2000, 40: 1035
[13] Reti T, Fried Z, Felde I.Computer simulation of steel quenching process using a multi-phase transformation model[J]. Comput. Mater. Sci., 2001, 22: 261
[14] Hong S C, Lim S H, Hong H S, et al.Effects of Nb on strain induced ferrite transformation in C-Mn steel[J]. Mater. Sci. Eng., 2003, A355: 241
[15] Adamczyk J, Kalinowska-Ozgowicz E, Ozgowicz W, et al.Interaction of carbonitrides V(C, N) undissolved in austenite on the structure and mechanical properties of microalloyed V-N steels[J]. J. Mater. Proc. Technol., 1995, 53: 23
[16] Hong S G, Kang K B, Park C G.Strain-induced precipitation of NbC in Nb and Nb-Ti microalloyed HSLA steels[J]. Scr. Mater., 2002, 46: 163
[17] Hong S G, Jun H J, Kang K B, et al.Evolution of precipitates in the Nb-Ti-V microalloyed HSLA steels during reheating[J]. Scr. Mater., 2003, 48: 1201
[18] Maropoulos S, Karagiannis S, Ridley N.The effect of austenitising temperature on prior austenite grain size in a low-alloy steel[J]. Mater. Sci. Eng., 2008, A483: 735
[19] Wang Y.Microstructure evolution and precipitation behaviors of second phase of X80 pipeline steels by hot charged processing [D].[D] Beijing: University of Science and Technology Beijing, 2010
[19] (王岩. 热送热装X80管线钢组织演变及第二相析出规律研究[D]. 北京: 北京科技大学, 2010)
[20] Poths R M, Higginson R L, Palmiere E J.Complex precipitation behavior in a microalloyed plate steel[J]. Scr. Mater., 2001, 44: 147
[21] Craver A J, He K, Garvie L A J, et al. Complex heterogeneous precipitation in titanium-niobium microalloyed Al-killed HSLA steels——I. (Ti, Nb)(C, N) particles[J]. Acta Mater., 2000, 48: 3857
[22] Yong Q L, Ma M T, Wu B R.Microalloyed Steels——Physical and Mechanical Metallurgy [M]. Beijing: Mechanical Industry Press, 1989: 254
[22] (雍岐龙, 马鸣图, 吴宝熔. 微合金钢——物理和力学冶金 [M]. 北京: 机械工业出版社, 1989: 254)
[23] Yoshie A, Fujioka M, Watanabe Y, et al.Modelling of microstructural evolution and mechanical properties of steel plates produced by thermo-mechanical control process[J]. ISIJ Int., 1992, 32: 395
[24] Zhong Y L, Liu G Q, Liu S X, et al.Austenite grain growth behavior of steel 33Mn2V designed for oil-well tubes[J]. Acta Metall. Sin., 2003, 39: 699
[24] (钟云龙, 刘国权, 刘胜新等. 新型油井管钢33Mn2V的奥氏体晶粒长大规律[J]. 金属学报, 2003, 39: 699)
[25] Gladman T.On the theory of the effect of precipitate particles on grain growth in metals[J]. Proc. Roy. Soc., 1966, 266A: 298
[26] Hillert M, Waldenstr?m M.A thermodynamic analysis of the Fe-Mn-C system[J]. Metall. Trans., 1977, 8: 5
[27] Saito Y, Shiga C.Computer simulation of microstructural evolution in thermomechanical processing of steel plates[J]. ISIJ Int., 1992, 32: 414
[28] Yang X L.Effects of heating temperature on solid solution of second phase particles and grain growth in pipeline steel[J]. Iron Steel Vanad. Titan., 2002, 23(2): 11
[28] (杨秀亮. 加热温度对管线钢第二相粒子固溶及晶粒长大的影响[J]. 钢铁钒钛, 2002, 23(2): 11)
[29] Xue R D, Zhao Z Y, Wang M X, et al.Effect of soaking time on the law of solid solution of Ti and Nb microalloyed high strength steel[J]. J Univ. Sci. Technol. Beijing, 2007, 29: 907
[29] (薛润东, 赵志毅, 王明侠等. 均热时间对含Ti、Nb 微合金元素高强钢固溶规律的影响[J]. 北京科技大学学报, 2007, 29: 907)
Outlines

/