APPLICATION OF HIGH RESOLUTION TRANSMISSION X-RAY TOMOGRAPHY IN MATERIAL SCIENCE

  • WANG Shaogang ,
  • WANG Sucheng ,
  • ZHANG Lei
Expand
  • Shenyang National Laboratory for Materials Science, Institute of Metal Research, Chinese Academy of Sciences, Shenyang 110016

Received date: 2013-03-06

  Revised date: 2013-06-04

  Online published: 2013-08-11

Abstract

The continuing development of X-ray light sources, optical devices and image analysis technologies enables us to nondestructively analyze internal structures of materials by using 3D imaging with a spatial resolution of micron, even dozens of nanometers. Innovations in materials science and technology will benefit from the new achievements of the X-ray tomography with higher resolution. This article devotes to review the origination and development of the X-ray tomography techniques for 3D imaging and introduce the principles and specifications of three imaging methods, including absorption imaging, phase contrast imaging and holographic imaging. The differences between synchrotron-based and laboratory-based X-ray tomography are also discussed. To explore new opportunities of the high resolution X-ray tomography in the development of material science and technology, particular emphasis is laid on the applications for traditional materials with a 3D view, such as the characterizations of holes, cracks, corrosion, composites, and in situ testing etc..

Cite this article

WANG Shaogang , WANG Sucheng , ZHANG Lei . APPLICATION OF HIGH RESOLUTION TRANSMISSION X-RAY TOMOGRAPHY IN MATERIAL SCIENCE[J]. Acta Metall Sin, 2013 , 49(8) : 897 -910 . DOI: 10.3724/SP.J.1037.2013.00107

References

[1] Salvo L, Cloetens P, Maire E, Zabler S, Blandin J J,Buffiere J Y, Ludwig W, Boller E, Bellet D, Josserond C.Nucl Instrum Meth, 2003; 200B: 273
[2] Mobus G, Inkson B J. Mater Today, 2007; 10: 18
[3] Epting W K, Gelb J, Litster S. Adv Funct Mater,2012; 22: 555 [4] Salvo L, Suery M, Marmottant A, Limodin N, Bernard D.C R Phys, 2010; 11: 641
[5] Withers P J. Mater Today, 2007; 10: 26
[6] Stock S R. Int Mater Rev, 1999; 44: 141
[7] Radon J. Ber Verh Sachs Ak Mn, 1917; 69: 262
[8] Cormack A M. J Appl Phys, 1963; 34: 2722
[9] Houndfield G N. Br J Radiol, 1973; 46: 1016
[10] Kalender W A. Phys Med Biol, 2006; 51: R29
[11] Copley D C, Eberhard J W, Mohr G A. J Miner Met Mater Soc, 1994; 46: 14
[12] Elliott J C, Dover S D. J Microsc--Oxford, 1982;126: 211
[13] Flannery B P, Deckman H W, Roberge W G, Damico K L.Science, 1987; 237: 1439
[14] Haddad W S, McNulty I, Trebes J E, Anderson E H, Levesque R A, Yang L. Science, 1994; 266: 1213
[15] Guvenilir A, Breunig T M, Kinney J H, Stock S R.Acta Mater, 1997; 45: 1977
[16] Nielsen S F, Poulsen H F, Beckmann F, Thorning C, Wert J A. Acta Mater, 2003; 51: 2407
[17] Stock S R. Int Mater Rev, 2008; 53: 129
[18] Maire E, Buffiere J Y, Salvo L, Blandin J J, Ludwig W,Letang J M. Adv Eng Mater, 2001; 3: 539
[19] Banhart J, Borbely A, Dzieciol K, Garcia--Moreno F, Manke I, Kardjilov N, Kaysser-Pyzalla A R, Strobl M, Treimer W.Int J Mater Res, 2010; 101: 1069
[20] Cazaux J, Erre D, Mouze D, Patat J M, Rondot S, Sasov A,Trebbia P, Zolfaghari A. J Phys IV, 1993; 3: 2099
[21] Mayo S C, Stevenson A W, Wilkins S W. Materials,2012; 5: 937
[22] Abbe S, Honorat P, Vincent M N. In: Nair C G K, Raj B,Nurthy C R L, Jayakumar T eds., Proc 14th world Conf on Non-Destruct Testing, Rotterdam: A. A. Balkema, 1996: 1397
[23] Allen A J. J Am Ceram Soc, 2005; 88: 1367
[24] Andersson L, Jones A C, Knackstedt M A, Bergstrom L.J Eur Ceram Soc, 2010; 30: 2547
[25] Appoloni C R, Macedo A, Fernandes C P, Philippi P C.X-Ray Spectrom, 2002; 31: 124
[26] Atwood R C, Jones J R, Lee P D, Hench L L. Scr Mater, 2004; 51: 1029
[27] Alemdar A, Zhang H, Sain M, Cescutti G, Mussig J.Adv Eng Mater, 2008; 10: 126
[28] Aldica G V, Nita P, Tiseanu I, Craciunescu T, Badica P.J Optoelectron Adv Mater, 2008; 10: 929
[29] Asghar Z, Requena G, Degischer H P, Cloetens P.Acta Mater, 2009; 57: 4125
[30] Dupuy L, Blandin J J. Acta Mater, 2002; 50: 3251
[31] Fabregue D, Deschamps A, Suery M, Proudhon H. ScrMater, 2008; 59: 324
[32] Gonazalez M, Dominguez G, Bathias C. J ComposTechnol Res, 2000; 22: 45
[33] Hamilton R W, Forster M F, Dashwood R J, Lee P D.Scr Mater, 2002; 46: 25
[34] Balla V K, Bose S, Bandyopadhyay A. Philos Mag,2010; 90: 3081
[35] Benouali A H, Froyen L, Delerue J F, Wevers M.Mater Sci Technol, 2002; 18: 489
[36] Caty O, Buffiere J Y, Maire E, Adrien J. Adv Eng Mater, 2011; 13: 194
[37] Lorthios J, Nguyen F, Gourgues A F, Morgeneyer T F, CugyP. Scr Mater, 2010; 63: 1220
[38] Puncreobutr C, Lee P D, Hamilton R W, Phillion A B.JOM, 2012; 64: 89
[39] Sinclair R, Preuss M, Maire E, Buffiere J Y, Bowen P,Withers P J. Acta Mater, 2004; 52: 1423
[40] Van Bael S, Kerckhofs G, Moesen M, Pyka G, Schrooten J,Kruth J P. Mater Sci Eng, 2011; A528: 7423
[41] Wang S G, Sun M Y, Song Z Q, Xu J.Intermetallics, 2012; 29: 123
[42] Adrien J, Maire E, Gimenez N, Sauvant--Moynot V.Acta Mater, 2007; 55: 1667
[43] Aroush D R B, Maire E, Gauthier C, Youssef S, Cloetens P,Wagner H D. Compos Sci Technol, 2006; 66: 1348
[44] Babout L, Maire E, Buffiere J Y, Fougeres R. Acta Mater, 2001; 49: 2055
[45] Babout L, Marrow T J, Engelberg D, Withers P J.Mater Sci Technol, 2006; 22: 1068
[46] Bareggi A, Maire E, Bouaziz O, Di Michiel M. Int J Fracture, 2012; 174: 217
[47] Bayraktar E, Garza M A G, Bathias C. J Mater Process Technol, 2008; 200: 133
[48] Berek H, Ballaschk U, Aneziris C G. Adv Eng Mater, 2011; 13: 1101
[49] Bernard D, Gendron D, Heintz J M, Bordere S, Etourneau J.Acta Mater, 2005; 53: 121
[50] Terzi S, Salvo L, Suery M, Dahle A K, Boller E.Acta Mater, 2010; 58: 20
[51] Long Y, Fessler J A, Balter J M. IEEE Trans Med Imaging, 2010; 29: 1839
[52] Attix F H. Radiation Dosimetry. 2 Ed., Salt Lake City: Academic Press, 1968: 405
[53] http:/ /www.nist.gov/pml/data/xraycoef/index.cfm
[54] Cloetens P, Ludwig W, Baruchel J, Van Dyck D, Van Landuyt J, Guigay J P, Schlenker M. Appl Phys Lett, 1999; 75: 2912
[55] Cloetens P, Ludwig W, Guigay J P, Baruchel J, Schlenker M, Van Dyck D. In: Baruchel J, Buffiere J Y, Maire E, Merle P, Peix G eds., X-Ray Tomography in Material Science. Paris: Hermes Science Publications, 2000: 29
[56] Beckmann F, Bonse U, Busch F, Gunnewig O. J Comput Assisted Tomography, 1997; 21: 539
[57] Snigirev A, Snigireva I, Kohn V, Kuznetsov S, Schelokov I. Rev Sci Instrum, 1995; 66: 5486
[58] Momose A, Fukuda J. Med Phys, 1995; 22: 375
[59] Takeda T, Momose A, Itai Y, Wu J, Hirano K. Acad Radiol, 1995; 2: 799
[60] Momose A, Takeda T, Itai Y, Hirano K. Nat Med,1996; 2: 473
[61] Bonse U, Hart M. Appl Phys Lett, 1965; 6: 155
[62] Forster E, Goetz K, Zaumseil P. Kristall Und Technik, 1980; 15: 937
[63] Momose A, Kawamoto S, Koyama I, Hamaishi Y, Takai K,Suzuki Y. Jpn J Appl Phys, 2003; 42: L866
[64] Ando M, Hosoya S. An Attempt at X-­­­­­Ray Phase-Contrast Microscopy. Tokyo: University of Tokyo Press, 1972:63
[65] Momose A. Opt Express, 2003; 11: 2303
[66] Cloetens P, Barrett R, Baruchel J, Guigay J P, Schlenker M. J Phys, 1996; 29D: 133
[67] Ingal V N, Beliaevskaya E A. J Phys, 1995; 28D:2314
[68] Dilmanian F A, Zhong Z, Ren B, Wu X Y, Chapman L D, Orion I, Thomlinson W C. Phys Med Biol, 2000; 45: 933
[69] David C, Nohammer B, Solak H H, Ziegler E. Appl Phys Lett, 2002; 81: 3287
[70] Pfeiffer F, Weitkamp T, Bunk O, David C. Nat Phys, 2006; 2: 258
[71] Wilkins S W, Gureyev T E, Gao D, Pogany A, Stevenson A W.Nature, 1996; 384: 335
[72] Cloetens P, Guigay J P, DeMartino C, Baruchel J, Schlenker M. Opt Lett, 1997; 22: 1059
[73] Talbot H F. Philos Mag, 1836; 9: 401
[74] Gibson L J. Annu Rev Mater Sci, 2000; 30: 191
[75] Maire E. Annu Rev Mater Sci, 2012; 42: 163
[76] Elmoutaouakkil A, Salvo L, Maire E, Peix G. Adv Eng Mater, 2002; 4: 803
[77] Fife J L, Li J C, Dunand D C, Voorhees P W. J Mater Res, 2009; 24: 117
[78] Chaijaruwanich A, Lee P D, Dashwood R J, Youssef Y M, Nagaumi H. Acta Mater, 2007; 55: 285
[79] Fonda R W, Lauridsen E M, Ludwig W, Tafforeau P, Spanos G.Metall Mater Trans, 2007; 38A: 2721
[80] Bouchard P O, Bourgeon L, Lachapele H, Maire E, Verdu C,Forestier R, Loge R E. Mater Sci Eng, 2008; A496: 223
[81] Lashkari O, Yao L, Cockcroft S, Maijer D. Metall Mater Trans, 2009; 40A: 991
[82] Youssef Y M, Chaijaruwanich A, Hamilton R W, Nagaumi H,Dashwood R J, Lee P D. Mater Sci Technol, 2006; 22: 1087
[83] Link T, Zabler S, Epishin A, Haibel A, Bansal A, Thibault X. Mater Sci Eng, 2006; A425: 47
[84] Weiler J P, Wood J T, Klassen R, Maire E, Berkmortel R,Wang G. Mater Sci Eng, 2005; A395: 315
[85] Khan S, Wilde F, Beckmann F, Mosler J. Int J Fatigue, 2012; 38: 92
[86] Zhang H, Toda H, Qu P C, Sakaguchi Y, Kobayashi M, Uesugi K, Suzuki Y. Acta Mater, 2009; 57: 3287
[87] Li P, Lee P D, Maijer D M, Lindley T C. Acta Mater, 2009; 57: 3539
[88] Hung Y C, Bennett J A, Garcia--Pastor F A, Di Michlel M,Buffiere J Y, Doel T J A, Bowen P, Withers P J. Acta Mater,2009; 57: 590
[89] Verdu C, Adrien J, Buffiere J Y. Mater Sci Eng,2008; A483-484: 402
[90] Xue Y, Pascu A, Horstemeyer M F, Wang L, Wang P T.Acta Mater, 2010; 58: 4029
[91] Buffiere J Y, Ferrie E, Proudhon H, Ludwig W.Mater Sci Technol, 2006; 22: 1019
[92] Ludwig W, Buffiere J Y, Savelli S, Cloetens P.Acta Mater, 2003; 51: 585
[93] Buffiere J Y, Savelli S, Jouneau P H, Maire E, Fougeres R.Mater Sci Eng, 2001; A316: 115
[94] Marrow T J, Buffiere J Y, Withers P J, Johnson G,Engelberg D. Int J Fatigue, 2004; 26: 717
[95] Clement P, Angeli J P, Pineau A. Fatigue Frat Eng Mater Struct, 1984; 7: 251
[96] Ferrie E, Buffiere J Y, Ludwig W. Int J Fatigue,2005; 27: 1215
[97] Knight S P, Salagaras M, Trueman A R. Corros Sci,2011; 53: 727
[98] Eckermann F, Suter T, Uggowitzer P J, Afseth A, Davenport A J, Connolly B J, Larsen M H, De Carlo F, Schmutz P. Corros Sci, 2008; 50: 3455
[99] Davenport A J, Padovani C, Connolly B J, Stevens N P C, Beale T A W, Groso A, Stampanoni M. Electrochem Solid State Lett, 2007; 10: C5
[100] Ghahari S M, Davenport A J, Rayment T, Suter T, Tinnes J P, Padovani C, Hammons J A, Stampanoni M, Marone F, Mokso R.Corros Sci, 2011; 53: 2684
[101] Horner D A, Connolly B J, Zhou S, Crocker L, Turnbull A. Corros Sci, 2011; 53: 3466
[102] Fuloria D, Lee P D, Bernard D. Mater Sci Eng,2008; A494: 3
[103] Dobrich K M, Rau C, Krill C E. Metall Mater Trans, 2004; 35A: 1953
[104] Wang M Y, Williams J J, Jiang L, De Carlo F, Jing T,Chawla N. Scr Mater, 2011; 65: 855
[105] Landron C, Maire E, Adrien J, Suhonen H, Cloetens P, Bouaziz O. Scr Mater, 2012; 66: 1077
[106] Qian L, Toda H, Uesugi K, Kobayashi T, Ohgaki T, Kobayashi M. Appl Phys Lett, 2005; 87: 241907
[107] Scheck C, Zupan M. Scr Mater, 2011; 65: 1041
[108] Birosca S, Buffiere J Y, Garcia-Pastor F A, Karadge M, Babout L, Preuss M. Acta Mater, 2009; 57: 5834
[109] Buffiere J Y, Maire E, Cloetens P, Lormand G, Fougeres R. Acta Mater, 1999; 47: 1613
[110] Beckmann F, Grupp R, Haibel A, Huppmann M, Noethe M, Pyzalla A, Reimers W, Schreyer A, Zettler R. Adv Eng Mater,2007; 9: 939
[111] Maire E, Carmona V, Courbon J, Ludwig W. Acta Mater, 2007; 55: 6806
[112] Gammage J J, Wilkinson D S, Embury J D, Maire E. Philos Mag, 2005; 85: 3191
[113] Limodin N, Salvo L, Boller E, Suery M, Felberbaum M, Gailliegue S, Madi K. Acta Mater, 2009; 57: 2300
[114] Baruchel J, Buffiere J Y, Cloetens P, Di Michiel M, Ferrie E, Ludwig W, Maire E, Salvo L. Scr Mater, 2006; 55:41
[115] Zhu P P, Wang J Y, Yuan Q X, Huang W X, Shu H, Gao B, Hu T D, Wu Z Y. Appl Phys Lett, 2005; 87: 264101
[116] Wang J Y, Zhu P P, Yuan Q X, Huang W X, Shu H, Chen B, Hu T D, Wu Z Y. Phys Med Biol, 2006; 51: 3391
[117] Huang Z F, Kang K J, Li Z, Zhu P P, Yuan Q X, Huang W X, Wang J Y, Zhang D, Yu A M. Appl Phys Lett, 2006; 89: 041124
[118] Zhu P P, Yuan Q X, Huang W X, Wang J Y, Shu H, Chen B, Liu Y J, Li E R, Wu Z Y. J Phys, 2006; 39D: 4142
[119] Egbert A, Brunke O. In: Medvids As ed., Int Academia 2010: Global Research and Education, Zurich: Trans Tech Publications, 2011: 48
[120] Kastner J, Harrer B, Degischer H P. Mater Charact, 2011; 62: 99
[121] Connolly B J, Horner D A, Fox S J, Davenport A J,Padovani C, Zhou S, Turnbull A, Preuss M, Stevens N P, Marrow T J, Buffiere J Y, Boller E, Groso A, Stampanoni M. Mater Sci Technol, 2006; 22: 1076
[122] Gebert J M, Wanner A, Piat R, Guichard M, Rieck S,Paluszynski B, Bohlke T. Mech Adv Mater Struct, 2008; 15:467
[123] Jakubek J, Granja C, Dammer J, Hanus R, Holy T, Pospisil S, Tykva R, Uher J, Vykydal Z. Nucl Instrum Meth, 2007;571A: 69
[124] Engelhardt M, Baumann J, Schuster M, Kottler C, Pfeiffer F, Bunk O, David C. Appl Phys Lett, 2007; 90: 224101
[125] Kashyap Y S, Yadav P S, Roy T, Sarkar P S, Shukla M, Sinha A. Appl Radiat Isotopes, 2008; 66: 1083
[126] Kastner J, Plank B, Requena G. Mater Charact,2012; 64: 79
[127] Ignatyev K, Munro P R T, Speller R D, Olivo A. In:McNulty I, Eyberger C, Lai B eds., 10th Int Conf on X-Ray Microscopy, New York: Amer Inst Physics, 2011: 254
[128] Mayo S C, Davis T J, Gureyev T E, Miller P R, Paganin D,Pogany A, Stevenson A W, Wilkins S W. Opt Express, 2003;11: 2289
[129] Limodin N, Rethore J, Buffiere J Y, Gravouil A, Hild F,Roux S. Acta Mater, 2009; 57: 4090
[130] Gao D Z, Ma X J, Jia P, Ye C G. High Power Laser Part Beams, 2010; 22: 2331
(高党忠, 马小军, 贾鹏, 叶成钢. 强激光与离子束, 2010; 22:2331)
[131] Gao H L, Shen Y, Xu J. J Mater Res, 2011; 26:2087
[132]http:/ /www.tms.org/Meetings/Specialty/3D2012/home.aspx
[133] Ludwig W, King A, Reischig P, Herbig M, Lauridsen E M,Schmidt S, Proudhon H, Forest S, Cloetens P, du Roscoat S R,Buffiere J Y, Marrow T J, Poulsen H F. Mater Sci Eng, 2009;A524: 69

Outlines

/

〈 〉