论文

DIRECTIONAL SOLIDIFICATION OF Ti–43Al–3Si ALLOYS IN AN OPTICAL FLOATING ZONE FURNACE

  • LIU Rong-Hua ,
  • TENG Chun-Yu ,
  • CUI Yu-You ,
  • XU Dong-Sheng ,
  • XIAN Quan-Gang ,
  • YANG Rui
Expand
  • Institute of Metal Research, Chinese Academy of Sciences, Shenyang 110016

Received date: 2011-09-29

  Revised date: 2011-11-01

  Online published: 2012-02-11

Abstract

Directional solidification (DS) process of Ti–43Al–3Si alloys in an optical floating zone furnace has been studied. The Φ9 mm polycrystalline rods with appropriate microstructure were cut from Φ70 mm cast ingot and used as seeds. At a growth rate of 5 mm/h, the DS ingot with lamellar structure parallel to longitudinal axis was obtained. The results of OM show that in the L+α+β three–phase region, the central α phase was successfully seeding by the polycrystalline rods and gradually develops into a dominant microstructure under a bent solid–liquid interface. The selection of polycrystalline seed, principle of three–phase region and bent solid–liquid interface directional solidification were discussed in detail.

Cite this article

LIU Rong-Hua , TENG Chun-Yu , CUI Yu-You , XU Dong-Sheng , XIAN Quan-Gang , YANG Rui . DIRECTIONAL SOLIDIFICATION OF Ti–43Al–3Si ALLOYS IN AN OPTICAL FLOATING ZONE FURNACE[J]. Acta Metall Sin, 2012 , 48(2) : 235 -239 . DOI: 10.3724/SP.J.1037.2011.00620

References

[1] Yamaguchi M, Inui H. In: Darolia R, Lweandowski J J, Liu C T, Martin P L, Miracle D B, Nathal M V, eds.. Structural Intermetallics. Warrendale, PA: TMS; 1993: 127

[2] Dimiduk D M. Mater Sci Eng, 1999; A263: 281

[3] Nazmy M, Staubli M, Onofrio G, Lupinc V. Scr Mater, 2001; 45: 787

[4] Evangelista E, Zhang W J, Francesconi L, Nazmy M. Scr Metall Mater, 1995; 33: 467

[5] Yamaguchi M, Inui H, Ito K. Acta Mater, 2000; 48: 307

[6] Inui H, Kishida K, Kobayashi M, Shirai Y, Yamaguchi M. Philos Mag, 1995; 72: 1609

[7] Johnson D R, Masuda Y, Inui H, Yamaguchi M. Metall Transrm, 2000; 31A: 2463

[8] Lee H N, Johnson D R, Inui H, Oh M H,Wee D M, Yamaguchi M. Intermetallics, 2002; 10: 841

[9] Johnson D R, Inui H, Yamaguchi M. Acta Mater, 1996; 44: 2523

[10] Johnson D R, Masuda Y, Inui H, Yamaguchi M. Acta Mater, 1997; 45: 2523

[11] Kim M C, Oh M H, Lee J H, Inui H, Yamaguchi M, Wee D M. Mater Sci Eng, 1997; A239–240: 570

[12] Kim S E, Lee Y T, Oh M H, Inui H, Yamaguchi M. Mater Sci Eng, 2002; A329–331: 25

[13] Johnson D R, Masuda Y, Inui H, Yamaguchi M. Mater Sci Eng, 1997; A329–240: 577

[14] Kim S E, Lee Y T, Oh M H, Inui H, Yamaguchi M. Intermetallics, 2000; 8: 399

[15] Jung I S, Jang H S, Oh M H, Lee J H, Wee D M. Mater Sci Eng, 2002; A329–331: 13

[16] Muto S,Yamanaka T, Johnson D R, Inui H, Yamaguchi M. Mater Sci Eng, 2002; A329–331: 424

[17] Johnson D R, Inui H, Muto S, Omiya Y, Yaamanaka T. Acta Mater, 2006; 54: 1077

[18] Luo W Z, Shen J, Li Q L, Man W W, Zhen X Q, Liu L, Fu H Z. Acta Metall Sin, 2006; 42: 1238

(罗文忠, 沈军, 李庆林, 满伟伟, 郑循强, 刘林, 傅恒志. 金属学报, 2006; 42: 1238)

[19] Luo W Z, Shen J, Li Q L, Man W W, Fu H Z. Acta Metall Sin, 2007; 43: 897

(罗文忠, 沈军, 李庆林, 满伟伟, 傅恒志. 金属学报, 2007; 43: 897)

[20] Luo W Z, Shen J, Li Q L, Fu H Z. Acta Metall Sin, 2007; 43: 1287

(罗文忠, 沈军, 李庆林, 傅恒志. 金属学报, 2007; 43: 1287)

[21] Lee J H, Yum J T, Choi K J, Lee J H, Choi SJ, Kor J. Inst Met Mater, 1997; 35: 712

[22] Yamaguchi M, Johnson D R, Lee H N, Inui H. Intermetallics, 2000; 8: 511

[23] Fu H Z, Guo J J, Su Y Q, Liu L, Xu D, Li J S. Chin J Nonferrous Met, 2003; 13: 797

(傅恒志, 郭景杰, 苏彦庆, 刘 林, 徐达鸣, 李金山. 中国有色金属学报, 2003; 13: 797)

[24] Liu R H, Cui Y Y, Yang R. Rare Met Mater Eng, 2008; 37(suppl3): 141

 (刘荣华, 崔玉友, 杨锐. 稀有金属材料与工程, 2008; 37(增刊3): 141)
Outlines

/

〈 〉