| Influence of Cr Micro-Addition on the Glass Forming Ability and Corrosion Resistance of Cu--Based Bulk Metallic Glasses |
| LIU Bing; LIU Lin ;SUN Min; QIU Chunlei; CHEN Qi |
| The State Key Laboratory of Plastic Forming Stimulation and Die & Mould Technology; Department of Materials Science and Technology; Huazhong University of Science and Technology; Wuhan 430074 |
|
Cite this article:
LIU Bing; LIU Lin; SUN Min; QIU Chunlei; CHEN Qi. Influence of Cr Micro-Addition on the Glass Forming Ability and Corrosion Resistance of Cu--Based Bulk Metallic Glasses. Acta Metall Sin, 2005, 41(7): 738-742 .
|
|
|
Abstract Cu47Zr11Ti34Ni8)100-xCrx(x=0, 0.5 and 1.0)
bulk metallic glasses (BMGs)
were obtained by water--cooled copper mold casting.
The effect of Cr micro--addition on the glass--forming ability
(GFA) of the alloys was investigated
by means of XRD, DSC and DTA. It was found
that Cr micro--addition can enhance the GFA.
Electrochemical measurements were carried out in 1 mol/L HCl,
3% NaCl and 6 mol/L KOH aqueous solutions by potentiadynamic
polarization method at room temperature. It
is shown that all the BMGs exhibited spontaneous
passivation in the above electrolytes, and with the increase of
Cr content, the passive zone remarkably increased and the passive
current density decreased, implying better
corrosion resistance of Cu-based BMGs with higher
Cr content. The present results also demonstrated that the
corrosion resistance of Cu--based BMGs with Cr micro--addition
is much better than that of the stainless steel.
|
|
Received: 04 November 2004
|
|
|
[1] Lin X H, Johnson W L. J Appl Phys, 1995; 78: 6514 [2] Inoue A, Zhang W, Zhang T, Kurosaka K. J Non-Cryst Solids, 2002; 304: 200 [3] Inoue A, Zhang W, Zhang T, Kurosaka K. Acta Mater, 2001; 49: 2645 [4] Choi-Yim H, Busch R, Johnson W L. J Appl Phys, 1998; 83: 7993 [5] Li C F, Saida J, Matsushida M, Inoue A. Scr Mater, 2000; 42: 923 [6] Zhang Q S, Zhang H F, Deng Y F, Ding B Z, Hu Z Q. Scr Mater, 2003; 49: 273 [7] Zhang T, Yamamoto T, Inoue A. Mater Trans JIM, 2002; 43: 3222 [8] Qin C L, Asami K, Zhang T, Inoue A. Mater Trans JIM, 2003; 44: 1042 [9] Qin C L, Asami K, Zhang T, Inoue A. Mater Trans JIM, 2003; 44: 749 [10] Yamamoto T, Zhang T, Inoue A. Mater Trans JIM, 2003; 44: 1147 [11] Inoue A. Bulk Amorphous Alloy: Preparation and Fundamental Characteristics. Switzerland: Trans Tech Pub- lication LTD, 1998: 37 [12] Zhang T, Inoue A. Mater Trans JIM, 1998; 39: 857 [13] Lu Z P, Li Y, Ng S C. J Non-Cryst Solids, 2000; 270: 103 [14] Inoue A, Zhang W, Zhang T, Kurosaka K. Acta Mater, 2001; 49: 2645 [15] Theodore A, Schroers W J, Johnson W L. Appl Phys Lett, 2001; 78: 1213 [16] Madge S V, Greer A L. Mater Sci Eng, 2004; A375: 759 [17] Huang J Z, Zuo Y. Corrosion Resistance Properties and Corrosion Data of Materials. Beijing: Chemical Industry Press, 2003: 45 (黄建中,左 禹.材料的耐蚀性和腐蚀数据.北京:化学工业 出版社,2003:345) [18] Turnbull D. Contemp Phys, 1969; 10: 473 [19] Johnson W L. MRS Bull, 1999; 10: 42 [20] de Boer F R, Boom R, Mattens W C M, Miedema A R, Niessen A K.' Cohesion in Metals. Amsterdam: NorthHolland, 1988: 179 [21] Luborsky F E. Amorphous Metallic Alloys. London: Butterudorths, 1983: 636 [22] Habazaki H, Ukai H, Izumiya K, Hashimoto K. Mater Sci Eng, 2001; 318A: 77 [23] Pang S J, Zhang T, Asami K, Inoue A. Corros Sci, 2002; 44: 1847 [24] Yao H B, Li Y, Wee A T S. Electrochim Acta, 2003; 48: 2641 [25] Beverskog B, Puigdomenech I. Corros Sci, 1997; 39: 43 |