Y元素对Cu-Al-Ni高温形状记忆合金性能的影响
收稿日期: 2021-09-16
修回日期: 2021-11-10
网络出版日期: 2021-12-09
基金资助
国家自然科学基金项目(52071236);天津市自然科学基金项目(18JCYBJC87000)
Effect of Y Element on the Properties of Cu-Al-Ni High Temperature Shape Memory Alloy
Received date: 2021-09-16
Revised date: 2021-11-10
Online published: 2021-12-09
Supported by
National Natural Science Foundation of China(52071236);Natural Science Foundation of Tianjin(18JCYBJC87000)
利用XRD、OM、SEM、TEM、电子万能力学试验机以及电化学工作站对Cu-13Al-4Ni-xY (x = 0.2、0.5,质量分数,%)高温形状记忆合金进行组织观察和性能测试。研究结果表明,加入Y元素后,Cu-13Al-4Ni-xY合金的室温组织主要为18R马氏体基体,以及具有六方结构的(Cu, Al, Ni)4Y第二相。随着Y元素含量的提高,Cu-13Al-4Ni-xY合金的力学性能大幅提升。当Y含量为0.5%时,压缩断裂应变与断裂强度从未添加Y时的10.5%和580 MPa分别提升到了19.3%和1185 MPa,且合金的断裂形式由沿晶断裂变为穿晶断裂。电化学实验结果表明,Y元素的添加使合金耐蚀性稍有下降。
张鑫 , 崔博 , 孙斌 , 赵旭 , 张欣 , 刘庆锁 , 董治中 . Y元素对Cu-Al-Ni高温形状记忆合金性能的影响[J]. 金属学报, 2022 , 58(8) : 1065 -1071 . DOI: 10.11900/0412.1961.2021.00400
Cu-Al-Ni alloys are not yet widely used due to issues related to their coarse grains, unacceptable plasticity, and poor thermal stability. Here, the physical and mechanical properties, as well as the corrosion behavior, of Cu-Al-Ni alloys doped with Y element (Cu-13Al-4Ni-xY (x = 0.2, 0.5, mass fraction, %)) were studied. XRD, OM, SEM, TEM, electronic universal testing machine, and electrochemical workstation were used to characterize the microstructures and measure the properties of the Cu-13Al-4Ni-xY alloys. The results showed that at room temperature, the microstructure of Cu-13Al-4Ni-xY alloys was mainly an 18R martensite matrix. The (Cu, Al, Ni)4Y second phase was characterized to have a hexagonal structure. The mechanical properties of the Cu-13Al-4Ni-xY alloys improved as the Y element content increased. For example, when the Y content was increased from 0% to 0.5%, the compressive fracture strain increased from 10.5% to 19.3% and the fracture strength increased from 580 to 1185 MPa. Additionally, the fracture type of the alloy changed from intergranular to transgranular with the addition of Y. Finally, the results from electrochemical experiments showed that the corrosion behavior of the alloys decreased slightly with the addition of Y.
| 1 | Zuo S G, Jin X J, Jin M J. Research progress in high temperature shape memory alloys [J]. Mater. Mech. Eng., 2014, 38(1): 1 |
| 1 | 左舜贵, 金学军, 金明江. 高温形状记忆合金的研究进展 [J]. 机械工程材料, 2014, 38(1): 1 |
| 2 | Zou Q, Dang S, Li Y G, et al. Research Progress of iron-based shape memory alloys: A review [J]. Mater. Rep., 2019, 33: 3955 |
| 2 | 邹 芹, 党 赏, 李艳国 等. Fe基形状记忆合金的研究进展 [J]. 材料导报, 2019, 33: 3955 |
| 3 | Zhang Y, Zeng H Y, Zhou J P, et al. Characterization of laser beam offset welding TiNi alloy and 304 stainless steel with different joining modes [J]. Opt. Laser Technol., 2020, 131: 106372 |
| 4 | Bellini C, Berto F, Di Cocco V, et al. A cyclic integrated microstructural-mechanical model for a shape memory alloy [J]. Int. J. Fatigue, 2021, 153: 106473 |
| 5 | Karaca H E, Acar E, Tobe H, et al. NiTiHf-based shape memory alloys [J]. Mater. Sci. Technol., 2014, 30: 1530 |
| 6 | Firstov G S, Van Humbeeck J, Koval Y N. High-temperature shape memory alloys [J]. Mater. Sci. Eng., 2003, A378: 2 |
| 7 | Firstov G S, Humbeeck J V, Koval Y N. High temperature shape memory alloys problems and prospects [J]. J. Intell. Mater. Syst. Struct., 2006, 17: 1041 |
| 8 | Hsieh S F, Chen S L, Lin H C, et al. The machining characteristics and shape recovery ability of Ti-Ni-X (X = Zr, Cr) ternary shape memory alloys using the wire electro-discharge machining [J]. Int. J. Mach. Tool Manuf., 2009, 49: 509 |
| 9 | Shamsolhodaei A, Panton B, Michael A, et al. Laser alloying as an effective way to fabricate NiTiPt shape memory alloys [J]. Metall. Mater. Trans., 2021, 52A: 4368 |
| 10 | Tong Y X, Chen F, Tian B, et al. Microstructure and martensitic transformation of Ti49Ni51 - x Hf x high temperature shape memory alloys [J]. Mater. Lett., 2009, 63: 1869 |
| 11 | Zhang X, Sui J H, Cai W, et al. Deformation mechanism of Ni54Mn25Ga20.9Gd0.1 high-temperature shape memory alloy [J]. Intermetallics, 2015, 67: 52 |
| 12 | Shao P, Ding L P, Luo D B, et al. Structural, electronic and elastic properties of the shape memory alloy NbRu: First-principle investigations [J]. J. Alloys Compd., 2017, 695: 3024 |
| 13 | Fonda R W, Jones H N, Vandermeer R A. The shape memory effect in equiatomic TaRu and NbRu alloys [J]. Scr. Mater., 1998, 39: 1031 |
| 14 | Gastien R, Corbellani C E, Sade M, et al. Thermal and pseudoelastic cycling in Cu-14.1Al-4.2Ni (wt%) single crystals [J]. Acta Mater., 2005, 53: 1685 |
| 15 | Zhu M, Ye X S, Li C H, et al. Preparation of single crystal CuAlNiBe SMA and its performances [J]. J. Alloys Compd., 2009, 478: 404 |
| 16 | Saud S N, Hamzah E, Abubakar T, et al. Effects of Mn additions on the structure, mechanical properties, and corrosion behavior of Cu-Al-Ni shape memory alloys [J]. J. Mater. Eng. Perform., 2014, 23: 3620 |
| 17 | Sari U. Influences of 2.5wt% Mn addition on the microstructure and mechanical properties of Cu-Al-Ni shape memory alloys [J]. Int. J. Miner. Metall. Mater., 2010, 17: 192 |
| 18 | Tong Y X, Li S Y, Zhang D T, et al. High strength and high electrical conductivity CuMg alloy prepared by cryorolling [J]. Trans. Nonferrous. Met. Soc., 2019, 29: 595 |
| 19 | Canbay C A, Karagoz Z. Effects of annealing temperature on thermomechanical properties of Cu-Al-Ni shape memory alloys [J]. Int. J. Thermophys., 2013, 34: 1325 |
| 20 | Zare M, Ketabchi M. Effect of chromium element on transformation, mechanical and corrosion behavior of thermomechanically induced Cu-Al-Ni shape-memory alloys [J]. J. Therm. Anal. Calorim., 2017, 127: 2113 |
| 21 | Zhang X, Zhang M, Cui T Y, et al. The enhancement of the mechanical properties and the shape memory effect for the Cu-13.0Al-4.0Ni alloy by boron addition [J]. J. Alloys Compd., 2019, 776: 326 |
| 22 | Deng Z H, Yin H Q, Zhang C, et al. Microstructure and mechanical properties of Cu-12Al-6Ni with Ti addition prepared by powder metallurgy [J]. Mater. Sci. Eng., 2021, A803: 140472 |
| 23 | Chang S H, Liao B S, Gholami-Kermanshahi M. Effect of Co additions on the damping properties of Cu-Al-Ni shape memory alloys [J]. J. Alloys Compd., 2020, 847: 156560 |
| 24 | Zhang X, Sui J H, Liu Q S, et al. Effects of Gd addition on the microstructure, mechanical properties and shape memory effect of polycrystalline Cu-Al-Ni shape memory alloy [J]. Mater. Lett., 2016, 180: 223 |
| 25 | Zhang X, Cui T Y, Zhang X, et al. Effect of Nd addition on the microstructure, mechanical properties, shape memory effect and corrosion behaviour of Cu-Al-Ni high-temperature shape memory alloys [J]. J. Alloys Compd., 2021, 858: 157685 |
| 26 | Stanciu S, Bujoreanu L G. Formation of stress-induced martensite in the presence of γ-phase, in a Cu-Al-Ni-Mn-Fe shape memory alloy [J]. Mater. Sci. Eng., 2008, A481-482: 494 |
| 27 | Badawy W A, El-Rabiee M M, Helal N H, et al. Effect of nickel content on the electrochemical behavior of Cu-Al-Ni alloys in chloride free neutral solutions [J]. Electrochim. Acta, 2010, 56: 913 |
| 28 | Lee J S, Wayman C M. Grain refinement of a Cu-Al-Ni shape memory alloy by Ti and Zr additions [J]. Trans. Jpn Inst. Met., 1986, 27: 584 |
| 29 | Chang S H, Kuo C, Han J L. Selective leaching and surface properties of Cu-Al-Ni shape memory alloys [J]. Mater. Trans., 2018, 59: 787 |
/
| 〈 |
|
〉 |