Ti对Zr-Nb二元合金β结构稳定性和力学性能的影响
收稿日期: 2020-04-20
修回日期: 2020-08-25
网络出版日期: 2020-09-09
基金资助
国家重点研发计划项目(2017YFB0702401);国家自然科学基金项目(91860108);辽宁省自然科学基金项目(2019-KF-05-01)
Effect of Ti on β Structural Stability and Mechanical Properties of Zr-Nb Binary Alloys
Received date: 2020-04-20
Revised date: 2020-08-25
Online published: 2020-09-09
Supported by
National Key Research and Development Program of China(2017YFB0702401);National Natural Science Foundation of China(91860108);Natural Science Foundation of Liaoning Province of China(2019-KF-05-01)
利用团簇成分式方法设计了[Zr-Zr14](Zr, Nb)3系列二元合金,进而采用Ti替代部分Zr形成三元合金;采用真空铜模吸铸快冷技术制备合金棒材,利用XRD、OM、TEM等对其进行微观组织表征和力学性能测试。结果表明,随着Nb含量增加,Zr-Nb二元合金基体结构从hcp-α向bcc-β转变,β结构稳定的同时伴随有ω相析出。适量Ti添加可显著抑制ω相的析出,进一步改善了合金的β结构稳定性。其中,单相bcc-β合金[Ti-Zr14]Nb3 (Zr-17.37Nb-2.98Ti,质量分数,%)表现出低弹性模量(E=57 GPa)的同时具有最佳的力学性能(屈服强度σYS=557 MPa、延伸率δ=15.5%)。
关键词: Zr-Nb-Ti合金; 结构稳定性; 团簇成分式; 弹性模量; 力学性能
王明康 , 苑峻豪 , 刘宇峰 , 王清 , 董闯 , 张中伟 . Ti对Zr-Nb二元合金β结构稳定性和力学性能的影响[J]. 金属学报, 2021 , 57(1) : 95 -102 . DOI: 10.11900/0412.1961.2020.00125
Metastable bcc β-Zr alloys generally have low elastic modulus, magnetic susceptibility, good mechanical properties, corrosion resistance, and biocompatibility, which are ascribed to co-alloying of multiple elements to enhance the structural stability of the bcc-β phase. This work systematically investigated the effects of Nb and Ti elements on the structural stability of the bcc-β phase and mechanical properties of Zr-Nb-Ti alloys. Various binary [Zr-Zr14](Zr, Nb)3 alloy compositions were designed by the cluster formula approach, based on which Ti was substituted for the base Zr to form ternary alloys. Alloy rods were prepared by the copper-mold suction-cast method with vacuum protection. The microstructure and mechanical properties of the alloys were characterized using XRD, OM, and TEM etc. The results show that the crystal structures of the Zr-Nb binary alloys could change from hcp-α to bcc-β with increasing Nb content, whereas, the ω-phase always coexists with the β-phase. An appropriate amount of Ti addition can significantly inhibit the precipitation of ω, resulting in the further improvement of the stability of the β-phase. The single β-[Ti-Zr14]Nb3 (Zr-17.37Nb-2.98Ti, mass fraction, %) ternary alloy exhibited not only a low elastic modulus of E=57 GPa but also a good tensile property with a high yield strength of σYS=557 MPa and an elongation of δ=15.5%.
| 1 | Yamamoto A, Honma R, Sumita M. Cytotoxicity evaluation of 43 metal salts using murine fibroblasts and osteoblastic cells [J]. J. Biomed. Mater. Res., 1998, 39: 331 |
| 2 | Guo S F, Liu Z, Chan K C, et al. A plastic Ni-free Zr-based bulk metallic glass with high specific strength and good corrosion properties in simulated body fluid [J]. Mater. Lett., 2012, 84: 81 |
| 3 | Mantripragada V P, Lecka-Czernik B, Ebraheim N A, et al. An overview of recent advances in designing orthopedic and craniofacial implants [J]. J. Biomed. Mater. Res., 2013, 101A: 3349 |
| 4 | Li H F, Zhou F Y, Li L, et al. Design and development of novel MRI compatible zirconium-ruthenium alloys with ultralow magnetic susceptibility [J]. Sci. Rep., 2016, 6: 24414 |
| 5 | Pêcheur D, Lefebvre F, Motta A T, et al. Effect of irradiation on the precipitate stability in Zr alloys [J]. J. Nucl. Mater., 1993, 205: 445 |
| 6 | Geetha M, Singh A K, Asokamani R, et al. Ti based biomaterials, the ultimate choice for orthopaedic implants—A review [J]. Prog. Mater Sci., 2009, 54: 397 |
| 7 | Li Y H, Yang C, Zhao H D, et al. New developments of Ti-based alloys for biomedical applications [J]. Materials, 2014, 7: 1709 |
| 8 | Suyalatu, Nomura N, Oya K, et al. Microstructure and magnetic susceptibility of as-cast Zr-Mo alloys [J]. Acta Biomater., 2010, 6: 1033 |
| 9 | Yang H L, Kano S, Matsukawa Y, et al. Study on recrystallization and correlated mechanical properties in Mo-modified Zr-Nb alloys [J]. Mater. Sci. Eng., 2016, A661: 9 |
| 10 | ? Zuzjaková, Zeman P, Haviar S, et al. Thermal stability of structure, microstructure and enhanced properties of Zr-Ta-O films with a low and high Ta content [J]. Surf. Coat. Technol., 2018, 335: 95 |
| 11 | Pang C, Wang Q, Zhang R Q, et al. β Zr-Nb-Ti-Mo-Sn alloys with low Young??s modulus and low magnetic susceptibility optimized via a cluster-plus-glue-atom model [J]. Mater. Sci. Eng., 2015, A626: 369 |
| 12 | Cai S, Daymond M R, Khan A K, et al. Elastic and plastic properties of βZr at room temperature [J]. J. Nucl. Mater., 2009, 393: 67 |
| 13 | Kondo R, Nomura N, Suyalatu, et al. Microstructure and mechanical properties of as-cast Zr-Nb alloys [J]. Acta Biomater., 2011, 7: 4278 |
| 14 | Kondo R, Shimizu R, Nomura N, et al. Effect of cold rolling on the magnetic susceptibility of Zr-14Nb alloy [J]. Acta Biomater., 2013, 9: 5795 |
| 15 | Dey G K, Tewari R, Banerjee S, et al. Formation of a shock deformation induced ω phase in Zr-20Nb alloy [J]. Acta Mater., 2004, 52: 5243 |
| 16 | Srivastava D, Mukhopadhyay P, Banerjee S, et al. Morphology and substructure of lath martensites in dilute Zr-Nb alloys [J]. Mater. Sci. Eng., 2000, A288: 101 |
| 17 | Ikeda M, Miyazaki T, Doi S, et al. Phase constitution and heat treatment behavior of Zr-Nb alloys [J]. Mater. Sci. Forum, 2007, 561: 1435 |
| 18 | Dey G K, Tewari R, Banerjee S, et al. Formation of a shock deformation induced ω phase in Zr-20Nb alloy [J]. Acta Mater., 2004, 52: 5243 |
| 19 | Banerjee S, Krishnan R. Martensitic transformation in zirconium-niobium alloys [J]. Acta Metall., 1971, 19: 1317 |
| 20 | Dey G K, Singh R N, Tewari R, et al. Metastability of the β-phase in Zr-rich Zr-Nb alloys [J]. J. Nucl. Mater., 1995, 224: 146 |
| 21 | Jiang B B, Wang Q, Wen D H, et al. Effects of Nb and Zr on structural stabilities of Ti-Mo-Sn-based alloys with low modulus [J]. Mater. Sci. Eng., 2017, A687: 1 |
| 22 | Jiang B B, Wang Q, Li X N, et al. Structural stability of the metastable β-[(Mo0.5Sn0.5)-(Ti13Zr1)]Nb1 alloy with low Young's modulus at different states [J]. Metall. Mater. Trans., 2017, 48A: 3912 |
| 23 | Pang C, Jiang B B, Shi Y, et al. Cluster-plus-glue-atom model and universal composition formulas [cluster](glue atom)x for BCC solid solution alloys [J]. J. Alloys Compd., 2015, 652: 63 |
| 24 | Hong H L, Wang Q, Dong C, et al. Understanding the Cu-Zn brass alloys using a short-range-order cluster model: Significance of specific compositions of industrial alloys [J]. Sci. Rep., 2014, 4: 7065 |
| 25 | Wang Q, Ji C J, Wang Y M, et al. β-Ti alloys with low Young??s moduli interpreted by cluster-plus-glue-atom model [J]. Metall. Mater. Trans., 2013, 44A: 1872 |
| 26 | Weiss I, Semiatin S L. Thermomechanical processing of beta titanium alloys—An overview [J]. Mater. Sci. Eng., 1998, A243: 46 |
| 27 | Wang Q, Dong C, Liaw P K. Structural stabilities of β-Ti alloys studied using a new Mo equivalent derived from [β/(α+β)] phase-boundary slopes [J]. Metall. Mater. Trans., 2015, 46A: 3440 |
| 28 | Zhang J Y, Fan S, Hao Y L, et al. Influence of equiatomic Zr/Nb substitution on superelastic behavior of Ti-Nb-Zr alloy [J]. Mater. Sci. Eng., 2013, A563: 78 |
| 29 | Bagaryatskiy Y A, Nosova G I. On the crystalline structure and the nature of the ω-phase in titanium alloys with chrome [J]. Fiz. Met. Metalloved., 1962, 13: 415 |
| 30 | Sun F, Zhang J Y, Marteleur M, et al. Investigation of early stage deformation mechanisms in a metastable β titanium alloy showing combined twinning-induced plasticity and transformation-induced plasticity effects [J]. Acta Mater., 2013, 61: 6406 |
| 31 | Ping D H, Mitarai Y, Yin F X. Microstructure and shape memory behavior of a Ti-30Nb-3Pd alloy [J]. Scr. Mater., 2005, 52: 1287 |
| 32 | Banerjee S, Tewari R, Dey G K. Omega phase transformation-morphologies and mechanisms [J]. Z. Metallkd., 2006, 97: 963 |
/
| 〈 |
|
〉 |