连续玄武岩纤维增强铝基层状复合材料的制备与力学特性
作者简介 丁 浩,男,1995年生,硕士生
收稿日期: 2017-12-11
网络出版日期: 2018-06-14
基金资助
国家自然科学基金项目Nos.51771064、51401068和51501040
Fabrication and Mechanical Characteristics of Multi-Laminated Aluminum Matrix Composites Reinforcedby Continuous Basalt Fibers
Received date: 2017-12-11
Online published: 2018-06-14
Supported by
Supported by National Natural Science Foundation of China (Nos.51771064, 51401068 and 51501040)
将连续玄武岩纤维(continuous basalt fiber,CBF)二维编织布与Al-12Si合金箔交替叠层堆垛成三明治结构,再利用真空压力浸渗技术成功制备出高体积分数(65%)的连续玄武岩纤维增强铝基(CBF/Al)层状复合材料。研究了浸渗工艺对复合材料微观组织演变的影响规律,阐明了CBF/Al复合材料的层状结构形成机理,并评价了其力学性能。研究表明:在温度为660 ℃、压力为10 MPa条件下浸渗10 min可以获得全致密的CBF/Al复合材料,其微观组织呈现独特的层状结构,即玄武岩纤维在铝合金基体中呈现垂直交叉层状分布特征,玄武岩纤维与铝合金基体未发生明显的化学反应,且由于玄武岩纤维与铝合金基体之间发生了元素(如Al、Si等)互扩散而形成了良好的冶金结合界面。纤维非理想排布方式而导致的有效承载能力下降以及高温下玄武岩纤维断裂强度降低是CBF/Al层状复合材料未达到理想力学性能的关键因素。
丁浩 , 崔喜平 , 许长寿 , 李爱滨 , 耿林 , 范国华 , 陈俊锋 , 孟松鹤 . 连续玄武岩纤维增强铝基层状复合材料的制备与力学特性[J]. 金属学报, 2018 , 54(8) : 1171 -1178 . DOI: 10.11900/0412.1961.2017.00530
Continuous basalt fiber (CBF) is a new type of performance outstanding inorganic nonmetallic material. In comparison with carbon fibers, basalt fibers exhibit greater failure strain as well as better impact and fire resistance with less poisonous fumes and 50% cost reduction. It is also known that basalt fibers display higher mechanical properties, better chemical stability and superior thermal and electrical insulation as compared with glass fibers. Basalt fiber has been widely used as a reinforcing composite material for construction industry and for preparation of polymer matrix composites. As high-performance low-cost reinforcements, basalt fibers should have a great potential for strengthening metal matrix composites (MMCs) and reducing their preparation cost. However, so far, few reports focused on the investigation on metal matrix composites reinforced by continuous basalt fibers, especially for lack of feasible fabrication technologies. Thus, in the present work, two-dimensional continuous basalt fiber cloth and Al-12Si alloys foils were selected as raw materials and alternately stacked to obtain a sandwiched structure. Subsequently, vacuum pressure infiltration was utilized to fabricate aluminum matrix composites reinforced by continuous basalt fibers (CBF/Al) with volume fraction of 65% successfully. Influence of infiltration parameters on microstructure evolution of resulting aluminum matrix composites was investigated and formation mechanism of multi-layered structure of CBF/Al composite was clarified. Moreover, mechanical properties of the multi-layered CBF/Al composite were evaluated. The results showed that when the infiltration parameters were 660 ℃, 10 MPa and 10 min, fully dense CBF/Al composite could be achieved and the novel composite displayed a unique multi-layered structure, namely continuous basalt fibers in forms of cruciform crossing distributed within aluminum alloys matrix. It is noteworthy that no obvious chemical reaction happened between continuous basalt fibers and Al-12Si alloys, and sound metallurgical bonding interface between them was obtained due to the interdiffusion of Al and Si elements. Unfortunately, mechanical properties of multi-layered CBF/Al composite did not reach a desired level, which was attributed to (i) decreasing of effective load-carrying capacity due to the imperfect distribution manner of continuous basalt fibers and (ii) deteriorating of intrinsic mechanical properties at high temperature.
| [1] | Cao H L, Lang H J, Meng S H.Experimental research on the basic structure and properties of the continuous basalt fiber[J]. Hi-Tech Fiber Appl., 2007, 32(5): 8(曹海琳, 郎海军, 孟松鹤. 连续玄武岩纤维结构与性能试验研究[J]. 高科技纤维与应用, 2007, 32(5): 8) |
| [2] | Asadi A, Baaij F, Mainka H, et al.Basalt fibers as a sustainable and cost-effective alternative to glass fibers in sheet molding compound (SMC)[J]. Composites, 2017, 123B: 210 |
| [3] | Kuzmin K L, Gutnikov S L, Zhukovskaya E S, et al.Basaltic glass fibers with advanced mechanical properties[J]. J. Non-Cryst. Solids, 2017, 476: 144 |
| [4] | Inman M, Thorhallsson E R, Azrague K.A mechanical and environmental assessment and comparison of basalt fibre reinforced polymer (BFRP) rebar and steel rebar in concrete beams[J]. Energy Proc., 2017, 111: 31 |
| [5] | Fiore V, Scalici T, Di Bella G, et al.A review on basalt fibre and its composites[J]. Composites, 2015, 74B: 74 |
| [6] | Dhand V, Mittal G, Rhee K Y, et al.A short review on basalt fiber reinforced polymer composites[J]. Composites, 2015, 73B: 166 |
| [7] | Shen D J, Yang Q, Jiao Y, et al.Experimental investigations on reinforced concrete shear walls strengthened with basalt fiber-reinforced polymers under cyclic load[J]. Constr. Build Mater., 2017, 136: 217 |
| [8] | Li R, Gu Y Z, Zhang G L, et al.Radiation shielding property of structural polymer composite: Continuous basalt fiber reinforced epoxy matrix composite containing erbium oxide[J]. Compos. Sci. Technol., 2017, 143: 67 |
| [9] | Korol E, Tejchman J, Mróz Z.Experimental and numerical assessment of size effect in geometrically similar slender concrete beams with basalt reinforcement[J]. Eng. Struct., 2017, 141: 272 |
| [10] | Bhat T, Chevali V, Liu X, et al.Fire structural resistance of basalt fibre composite[J]. Composites, 2015, 71A: 107 |
| [11] | Akhlaghi F, Eslami-Farsani R, Sabet S M M. Synthesis and characteristics of continuous basalt fiber reinforced aluminum matrix composites[J]. J. Compos. Mater., 2013, 47: 3379 |
| [12] | Xie Y L, Wang M L, Ma N H, et al.Interface reaction and property of basalt fiber reinforced Al-based composites[J]. Foundry Technol., 2013, 34: 805(谢雨凌, 汪明亮, 马乃恒等. 玄武岩纤维增强铝基复合材料的界面反应及力学性能分析[J]. 铸造技术, 2013, 34: 805) |
| [13] | Tjong S C, Ma Z Y.Microstructural and mechanical characteristics of in situ metal matrix composites[J]. Mater. Sci. Eng., 2000, R29: 50 |
| [14] | Dhanashekar M, Kumar S V S. Squeeze casting of aluminium metal matrix composites-an overview[J]. Proc. Eng., 2014; 97: 412 |
| [15] | Teng F, Yu K, Luo J, et al.Microstructures and properties of Al-50%SiC composites for electronic packaging applications[J]. Trans. Nonferrous Met. Soc. China, 2016, 26: 2647 |
| [16] | Pucci M F, Seghini M C, Liotier P J, et al.Surface characterisation and wetting properties of single basalt fibres[J]. Composites, 2017, 109B: 72 |
| [17] | Iorio M, Santarelli M L, González-Gaitano G, et al.Surface modification and characterization of basalt fibers as potential reinforcement of concretes[J]. Appl. Sur. Sci., 2018, 427: 1248 |
| [18] | Li F Z, Li G C, Wang H M, et al.Research on properties on high temperature resistance of basalt fiber yarn[J]. J. Funct. Mater., 2013, 46: 3063(李福洲, 李贵超, 王浩明等. 玄武岩纤维纱线的耐高温性能研究 [J]. 功能材料, 2013, 46: 3063) |
| [19] | Sarasini F, Tirillò J, Seghini M C.Influence of thermal conditioning on tensile behaviour of single basalt fibres[J]. Composites, 2018, 132B: 77 |
/
| 〈 |
|
〉 |