论文

长期热老化对铸造奥氏体不锈钢组织和性能的影响

  • 李时磊 ,
  • 李树肖 ,
  • 王艳丽 ,
  • 王西涛
展开
  • 北京科技大学新金属材料国家重点实验室, 北京 100083
李时磊, 男, 1982年生, 博士生

收稿日期: 2010-05-24

  修回日期: 2010-07-08

  网络出版日期: 2010-10-11

基金资助

国家重点基础研究发展计划项目2006CB605005和国家高技术研究发展计划项目2008AA031702资助

EFFECT OF LONG TERM AGING ON THE MICROSTRUCTURE AND MECHANICAL PROPERTIES OF CAST AUSTENITIC STAINLESS STEELS

  • LI Shi-Lei ,
  • LI Shu-Xiao ,
  • YU Yan-Li ,
  • YU Xi-Shou
Expand
  • State Key Laboratory for Advanced Metals and Materials, University of Science and Technology Beijing, Beijing 100083

Received date: 2010-05-24

  Revised date: 2010-07-08

  Online published: 2010-10-11

Supported by

Supported by National Basic Research Program of China (No.2006CB605005) and High Technology Research and Development Program of China (No.2008AA031702)

摘要

将铸造奥氏体不锈钢在400℃下时效至104 h, 通过力学性能测试和组织观察, 分析了老化时间对力学性能和组织结构的影响. 结果表明: 铁素体相的体积分数随老化时间没有变化; 长期老化后材料的磁导率降低, 同时铁素体相的纳米压入硬度增加; 材料的Charpy冲击功随老化时间迅速下降, 冲击断口形貌也随之不断变化; 通过TEM观察发现, 铁素体相在长期老化后析出了弥散 的α'相和少量的G相, α'相是由铁素体发生调幅分解而生成的, 是导致铸造奥氏体不锈钢热老化脆化的主要原因.

本文引用格式

李时磊 , 李树肖 , 王艳丽 , 王西涛 . 长期热老化对铸造奥氏体不锈钢组织和性能的影响[J]. 金属学报, 2010 , 46(10) : 1186 -1191 . DOI: 10.3724/SP.J.1037.2010.00250

Abstract

In order to study the mechanism of mid–temperature thermal aging embrittlement in cast austenite stainless steel (CASS), the mechanical properties and microstructure were investigated of CASS which was aged at 400 ℃for 104 h. The results show that, no change in the ferrite content (volume fraction) was detected. After long term aging, the magnetic permeability of the CASS declined, bt the nano–hardness of ferrite phases increased. The Charpy impact energy decreased rapidly and the impact fracture morphologies changed with aging time. Large number of α' particles precipitated homogeneously in the ferrite phases of the CASS aged for 104 h. α′ precipittion produced by spinodal decomposition in ferrite was considered to the primary mechanism of thermal aging in CASS at mid-temperature. G phases were also observed n some positions of ferrite after long term aging.

参考文献

[1] Pumphrey P H, Akhurst K N. Mater Sci Tech-Lond, 1990; 6: 211 [2] Bonnet S, Bourgoin J, Champredonde J, Guttmann D, Guttmann M. Mater Sci Tech-Lond, 1990; 6: 221 [3] Hale G E, Garwood S J. Mater Sci Tech-Lond, 1990; 6: 230 [4] Miller M K, Bentley J. Mater Sci Tech-Lond, 1990; 6: 285 [5] Brown J E, Cerezo A, Godfrey T J, Hetherington M G, Smith G D W. Mater Sci Tech-Lond, 1990; 6: 293 [6] Auger P, Danoix F, Menand A, Bonnet S, Bourgoin J, Guttmann M. Mater Sci Tech-Lond, 1990; 6: 301 [7] Mathew M D, Lietzan L M, Murty K L, Shah V N. Mat Sci Eng A-Struct, 1999; 269: 186 [8] Kawaguchi S, Sakamoto N, Takano G, Matsuda F, Kikuchi Y, Mraz L. Nucl Eng Des, 1997; 174(3): 273 [9] Yamada T, Okano S, Kuwano H. J Nucl Mater, 2006; 350(1): 47 [10] Danoix F, Auger P, Blavette D. Microsc Microanal. 2004; 10(3): 349 [11] Wang Y L. PhD Thesis, University of Science and Technology Beijing, 2001. (王艳丽. 北京科技大学博士论文, 2001) [12] Bethmont M, Meyzaud Y, Soulat P. Int J Pres Ves Pip. 1996; 65(3): 211 [13] Chung H M, Leax T R. Mater Sci Tech-Lond, 1990; 6: 249 [14] Chung H M. . Int J Pres Ves Pip, 1992; 50(1-3): 179 [15] Vrinat M, Cozar R, Meyzaud Y. Scripta Mater, 1986; 20(8):1101
文章导航

/