带材厚度对Fe75.2Si13B8Cu1Nb2.8纳米晶软磁合金磁畴结构和高频磁性能的影响
施博文, 李艳辉, 冯拓, 王雨, 蒋丽, 于凤云, 杨陆, 张伟

Effect of Ribbon Thickness on Magnetic Domain Structures and High-Frequency Magnetic Properties of Fe75.2Si13B8Cu1Nb2.8 Nanocrystalline Soft Magnetic Alloy
SHI Bowen, LI Yanhui, FENG Tuo, WANG Yu, JIANG Li, YU Fengyun, YANG Lu, ZHANG Wei
表1 不同厚度Fe75.2Si13B8Cu1Nb2.8纳米晶带材的α-Fe平均晶粒尺寸和磁性能参数
Table 1 Average α-Fe grain size and magnetic properties of Fe75.2Si13B8Cu1Nb2.8 nanocrystalline alloys with different thicknesses
Alloy

t

µm

Dα-Fe

nm

Bs

T

Hc

A·m-1

μePcm / (W·kg-1)
100 kHz1 MHz0.2 T, 100 kHz0.2 T, 500 kHz
T151511.01.360.617000520067811
T191911.61.360.5165004100811017
T232311.41.350.51400029001081396