合金化调控Nb-Si基超高温合金强韧化与抗氧化性能的研究进展
李云龙, 张子润, 于君, 赵占勇, 林鑫, 白培康

Research Progress on Alloying Regulation of Strengthening, Toughening, and Oxidation Resistance in Nb-Si-Based Ultrahigh-Temperature Alloys
LI Yunlong, ZHANG Zirun, YU Jun, ZHAO Zhanyong, LIN Xin, BAI Peikang
表2 合金元素对Nb-Si基超高温合金氧化行为的影响对比[31,33,35,36,39,42,44~54,58,65~70]
Table 2 Comparisons of oxidation behavior of Nb-Si-based ultrahigh-temperature alloys modified by various alloying elements[31,33,35,36,39,42,44-54,58,65-70]

Alloying

element

Main oxide-scale featureProtective effectMain trade-off

Ti[65]

TiO2-containing composite scale, Ti-rich outer layer; can form denser layer at high temperature

Improves compactness at > 1100 oC

Poor efficacy at lower temperatures; clear temperature window

Zr[31,58]

ZrO2 particles/regions; improved continuity of inner SiO2 layerZrO2 fills defects, reduces porosity, stabilizes protective sublayerExcess Zr increases brittle silicide fraction and degrades mechanical balance

Mo[33]

Less porous at suitable content; excessive Mo introduces pores and fast-diffusion pathsOptimizes phase constitution and indirectly retards oxidation at appropriate levelsNarrow beneficial window; overaddition aggravates oxidation via pore formation

Cr[35,66-68,70]

Forms Cr2O3, CrNbO4, or Cr-enriched outer scale; promotes dense external protective layerEnhances compactness and slows inward oxygen diffusionOften sacrifices room temperature toughness

Al[35,68]

Forms relatively dense Al2O3-containing scale; suppresses loose Nb2O5 growthImproves scale continuity, compactness, and oxygen-barrier capabilityReduces Nbss continuity and lowers room-temperature toughness

Ta[39]

Slightly denser scale; in some systems, helps reduce severe scale disruptionIndirectly optimizes phase constitution and oxidation responseVery narrow optimum (~1%, atomic fraction); over-addition reverses the benefit

Hf[42,69]

HfO2-containing scale or dispersed Hf-rich oxides; denser and more adherent multilayer architecture containing scale or dispersed Hf

Markedly improves scale adhesion, suppresses spallation, stabilizes protective layers

Increases density and cost; excessive Hf complicates phase constitution

B[36,44]

Alters oxidation response mainly through microstructure/eutectic modification, not by forming a dominant oxideRefines microstructure and helps construct a more uniform oxidation pathwayVery narrow window; excess B increases silicide fraction, impairing toughness and oxidation balance

Rare-earth element[45-54]

Forms stable rare-earth oxides or complex oxides (e.g., ErNbO4); denser and more adherent scaleReactive element effect: improves adhesion, suppresses cracking/spallation, reduces oxygen diffusion, purifies interfacesEffective only at trace/low levels; over-addition forms coarse oxides/inclusions that degrade integrity