Ag替换CuZr-Ti-Cu-Al非晶合金性能的影响
蔡正清, 尹大伟, 杨靓, 王文祥, 王飞龙, 温永清, 马明臻

Effect of Ag Substitution of Cu on Properties of Zr-Ti-Cu-Al Amorphous Alloys
CAI Zhengqing, YIN Dawei, YANG Liang, WANG Wenxiang, WANG Feilong, WEN Yongqing, MA Mingzhen
表4 Zr55Ti3Cu32 - x Al10Ag x 非晶合金的腐蚀参数
Table 4 Corrosion potential (Ecorr), corrosion current density (icorr), and pitting potential (Epit) of Zr55Ti3Cu32 - x Al10Ag x BMGs
Solutionxicorr / (A·cm-2)Ecorr / mVEpit / mV
PBS05.10 × 10-7-427.9-36.2
1.51.04 × 10-7-426.7-296.7
22.12 × 10-7-582.1-212.7
2.52.15 × 10-7-463.9-275.6
SBF05.56 × 10-8-311.7-100.9
1.53.68 × 10-8-346.5-175.3
21.03 × 10-8-278.8-203.2
2.52.02 × 10-8-381.7-102.7