利用小角中子核磁散射分离研究AerMet100钢中纳米析出相的形貌和成分
柯于斌, 李彬, 段辉平

Morphology and Chemical Composition of Nanoprecipitate in AerMet100 Steel by Separation of the Nuclear and Magnetic Small-Angle Neutron Scattering Data
KE Yubin, LI Bin, DUAN Huiping
表2 AerMet100钢SANS核散射拟合结果
Table 2 Fitted structural parameters of nanoprecipitates from the nuclear SANS data of AerMet100 steel
SampleD / nmL / nmRHS / nmfV / %
CoNi_4541.15 ± 0.766.00 ± 1.275.95 ± 1.050.54 ± 0.15
CoNi_4822.02 ± 1.049.63 ± 0.876.68 ± 0.922.47 ± 0.34
CoNi_4862.37 ± 0.7510.6 ± 1.726.75 ± 0.783.25 ± 0.38
CoNi_4982.48 ± 0.9915.9 ± 2.947.07 ± 0.935.19 ± 0.68