表2 不同处理工艺下镁合金细化效果对比[71,80,82,84,86,87,90,93,96]
Table 2 Comparisons of magnesium alloy refining effects by various treatment processes[71,80,82,84,86,87,90,93,96]

Treatment

Process

Alloy

Casting conditionHolding time / minAverage grain size / μm

Improvement

rate / %

Ref.

UntreatedTreated
Mg-Zr refinerUHFP-TIGRMg-9Gd-3Y-0.5ZrSteel ladle5924254[80]
treatedRollingMg-10Gd-3Y-0.5ZrSteel ladle15866030[71]
RollingMg-0.5ZrSteel ladle3016214510[84]
FSPMg-3Nd-0.2Zn-0.6ZrSteel ladle1514011121[86]
ECAEMg-2Zn-0.1ZrMetallic mold-13111016[87]
Mg alloy meltIMSMg-0.1Zr-30321*12760[90]
treatedUSTMg-1.0Zr--2949465[93]
PMFMg-Gd-Y-ZrGraphite crucible-653743[96]