深潜器耐压壳用钛合金保载疲劳服役可靠性研究进展
|
|
张滨, 田达, 宋竹满, 张广平
|
Research Progress in Dwell Fatigue Service Reliability of Titanium Alloys for Pressure Shell of Deep-Sea Submersible
|
|
ZHANG Bin, TIAN Da, SONG Zhuman, ZHANG Guangping
|
|
表4 TC4、TC4 ELI及Ti62A钛合金室温保载疲劳性能[3,22,51,68,89]
|
Table 4 Dwell fatigue properties of TC4, TC4 ELI, and Ti62A titanium alloys at room temperature[3,22,51,68,89]
|
|
| Alloy | Microstructure | σmax / σs | σmax / MPa | Th / s | R | Ndf | Ref. |
|---|
| TC4 | Bimodal | 0.900 | - | 120 | 0.1 | 3700 | [68] | | TC4 | Bimodal | 0.950 | 765 | 1 | 0 | 25205 | [51] | | TC4 | Bimodal | 0.950 | 765 | 10 | 0 | 16722 | [51] | | TC4 ELI | - | 0.906 | - | 600 | 0 | 1315 | [3] | | TC4 ELI | - | 0.924 | - | 600 | 0 | 1060 | [3] | | TC4 ELI | - | 0.941 | - | 600 | 0 | 735 | [3] | | TC4 ELI | - | 0.959 | - | 120 | 0 | 456 | [3] | | TC4 ELI | - | 0.959 | - | 600 | 0 | 306 | [3] | | TC4 ELI | - | 0.959 | - | 900 | 0 | 379 | [3] | | TC4 ELI | - | 0.976 | - | 600 | 0 | 232 | [3] | | TC4 ELI | Equiaxed | 0.956 | 815 | 120 | 0 | 2373 | [89] | | TC4 ELI | Equiaxed | 0.956 | 815 | 120 | -1 | 238 | [89] | | TC4 ELI | Equiaxed | 0.956 | 815 | 120 | 0.5 | 761 | [89] | | Ti62A | Bimodal | 0.950 | 893 | 1 | 0 | 18092 | [22] | | Ti62A | Bimodal | 0.950 | 893 | 10 | 0 | 14534 | [22] |
|
|
|