增材制造镁合金技术现状与研究进展
|
|
唐伟能, 莫宁, 侯娟
|
Research Progress of Additively Manufactured Magnesium Alloys: A Review
|
|
TANG Weineng, MO Ning, HOU Juan
|
|
表3 文献中不同镁合金WAAM最优工艺参数[44,50~57]
|
Table 3 Optimized WAAM process parameters of Mg alloys in literatures[44,50-57]
|
|
| Method | Alloy | Wire feed rate | Travel speed | Peak current | Dwell time | Ar flow rate | Ref. |
|---|
| | m·min-1 | mm·min-1 | A | s | L·min-1 | | | TIG | AZ31 | 2.00 | 200 | 136 | - | 20 | [50] | | AZ61 | 0.82 | - | 130 | - | - | [51] | | AZ80 | 1.15 | 300 | 100-120 | 160 | 17-20 | [52,53] | | MIG/CMT | AZ31 | - | 600 | 350 | 180 | 18 | [54] | | AZ31 | - | 800 | 100 | 20 | 25 | [44] | | AZ61 | 1.8 | 270 | 68 | 90 | 18 | [56] | | AEX11 | 2.2 | 720 | 51 | - | 14 | [57] | | AZ91D | 12 | 600 | - | 180 | 15 | [55] |
|
|
|