增材制造镁合金技术现状与研究进展
|
|
唐伟能, 莫宁, 侯娟
|
Research Progress of Additively Manufactured Magnesium Alloys: A Review
|
|
TANG Weineng, MO Ning, HOU Juan
|
|
表1 文献中Mg与镁合金SLM过程参数优化情况[21~25,35~42]
|
Table 1 Optimized processing parameters of SLM examined for Mg and Mg alloys in literatures[21-25,35-42]
|
|
| Material | Laser power | Layer thickness | Hatch spacing | Scan rate | Relative density | Ref. |
|---|
| W | μm | μm | mm·s-1 | % | | | Mg | 90 | 30 | 100 | 100 | 96.13 | [36] | | AZ31 | 75 | 50 | 100 | 125 | > 99.50 | [37] | | AZ61 | 150 | 40 | 60 | 400 | 99.40 | [21] | | Mg-9Al | 15 | 50 | 80 | 20 | 82.00 | [35] | | AZ91D | 200 | 40 | 90 | 330 | 99.52 | [22] | | AZ91D | 50 | 30 | 30 | 200 | 98.10 | [38] | | ZK60 | 50 | 100 | 100 | 500 | 97.40 | [39] | | ZK60 | 50 | 20 | 80 | 600 | 98.00 | [40] | | WE43 | 300 | 30 | 40 | 1200 | 99.40 | [41] | | WE43 | 195 | 30 | 200 | 800 | 99.60 | [42] | | WE43 | 200 | 40 | 130 | 1100 | 99.70 | [23] | | GZ112K | 80 | 30 | 100 | 300 | 99.95 | [25] | | GWZ1031K | 80 | 30 | 100 | 200 | 97.85 | [24] |
|
|
|