基于不同 α / β 团簇式比例的Ti-Al-V合金的铸态组织和力学性能
朱智浩, 陈志鹏, 刘田雨, 张爽, 董闯, 王清

Microstructure and Mechanical Properties of As-Cast Ti-Al-V Alloys with Different Proportion of α / β Clusters
ZHU Zhihao, CHEN Zhipeng, LIU Tianyu, ZHANG Shuang, DONG Chuang, WANG Qing
表1 不同β团簇式个数n设计的合金化学成分以及Mo和Al当量、估算的液固两相区
Table 1 Designed compositions following different numbers of β units (n) and their Al- and Mo-equivalents and solidification ranges
Material codenComposition / (mass fraction, %)[Mo]eq[Al]eq∆TL-S / oC
n00Ti-7.45Al0.07.54.9
n11Ti-7.16Al-0.82V0.67.24.9
n22Ti-6.87Al-1.62V1.16.94.7
n33Ti-6.60Al-2.41V1.46.64.5
n44Ti-6.32Al-3.19V2.16.39.4
n55Ti-6.05Al-3.94V2.66.113.3
n77Ti-5.53Al-5.45V3.65.520.7
n88Ti-5.28Al-6.14V4.15.324.3
n1212Ti-4.30Al-8.87V5.94.331.8
n1717Ti-3.19Al-12.03V8.03.135.1