选区激光熔化NiTi形状记忆合金研究进展
|
|
杨超, 卢海洲, 马宏伟, 蔡潍锶
|
Research and Development in NiTi Shape Memory Alloys Fabricated by Selective Laser Melting
|
|
YANG Chao, LU Haizhou, MA Hongwei, CAI Weisi
|
|
表1 常用的SLM制备NiTi SMAs的工艺参数[8,9,23,24,26~57]
|
Table 1 Process parameters of SLM NiTi SMAs[8,9,23,24,26-57]
|
|
| Process parameter | P / W | v / (mm·s-1) | h / mm | t / μm | E / (J·mm-3) | Ref. |
|---|
| characteristic | | | | | | | | High P with high v | 200-375 | 1000-1400 | 60 | 30 | 79-208 | [26] | | 250 | 1250 | 120 | 30 | 55.5 | [27-34] | | 200 | 1500 | 40-80 | 40 | 42-83 | [35] | | 250 | 900-1100 | 60-75 | 30 | 123-126 | [36] | | 250 | 1100 | 120 | 30 | 63 | [37] | | Low P with low v | 50-120 | 100-300 | 45-150 | 20 | 55-675 | [9] | | 70 | 105 | 100 | 30 | 222 | [23] | | 120 | 250 | 50 | 40 | 240 | [24] | | 40 | 160-280 | 50 | 30 | 95-111 | [36] | | 60-120 | 150-600 | 75 | 30 | 44-267 | [8,38] | | 90 | 600 | 90 | 30 | 56 | [39] | | 120 | 500 | 80 | 30 | 110 | [40-43] | | 90 | 414 | 120 | 30 | 61 | [44] | | 70 | 80-300 | 100 | 30 | 78-292 | [45-47] | | 50 | 200-300 | 120 | 30 | 46-69 | [48] | | 60 | 300-480 | 110 | 25 | 46-73 | [49,50] | | 50, 100 | 125 | 40-240 | 30 | 56-667 | [51] | | 110, 120 | 150-350 | 50 | 30 | 210-533 | [52] | | Other | 120 | 800 | 110 | 30 | 46 | [53] | | 50-250 | 250-1250 | 80-120 | 30 | 40-125 | [54] | | 75-200 | 400-1200 | 80-120 | 20-40 | 47-87 | [55,56] | | 60-240 | 500 | 80 | 30 | 50-200 | [57] |
|
|
|