砂型3DP打印参数对ZL205A合金铸造性能的影响
王春辉, 杨光昱, 阿热达克·阿力玛斯, 李晓刚, 介万奇

Effect of Printing Parameters of 3DP Sand Mold on the Casting Performance of ZL205A Alloy
WANG Chunhui, YANG Guangyu, ALIMASI Aredake, LI Xiaogang, JIE Wanqi
表2 不同3DP砂型打印参数下的ZL205A合金铸造性能实验值与拟合值
Table 2 Experimental and fitted values of the foundry properties for the ZL205A alloy prepared by 3DP sand mold with different printing parameters
X1X2Y1Y2ZY1*Y2*Z*∣Z*-Z∣ / Z
%mmmmmm%
1.50.28411850.9784.1171193.4211.002642.54
1.50.30211750.9591.8131172.0750.949290.97
1.50.32010700.621-0.2751066.8090.643381.25
2.00.285011700.67747.0031163.5370.673830.43
2.00.301811600.82423.9481146.4610.751068.88
2.00.32410650.6143.0531081.6000.669719.05
2.50.289011050.25791.5411088.8370.2000422.30
2.50.305010500.31346.9371069.9040.3933725.60
2.50.32610200.4676.5091015.5430.450333.50
3.00.28010900.7120.1631100.2410.742254.23
3.00.30010800.682-0.2281086.0690.700702.77
3.00.32010600.621-0.5821045.6070.250836.50