变形速率对GH3625合金弹-塑性变形行为的影响
高钰璧, 丁雨田, 李海峰, 董洪标, 张瑞尧, 李军, 罗全顺

Effect of Deformation Rate on the Elastic-Plastic Deformation Behavior of GH3625 Alloy
GAO Yubi, DING Yutian, LI Haifeng, DONG Hongbiao, ZHANG Ruiyao, LI Jun, LUO Quanshun
表5 不同变形速率下GH3625合金压缩变形后的ρ、ρGND和统计存储位错密度(ρSSD) (1014 m-2)
Table 5 ρ, ρGND, and statistically stored dislocation density (ρSSD) of GH3625 alloy after compression deformation under different rates
r / (mm·min-1)ρρGNDρSSD
0.218.48 ± 1.8111.337.15 ± 1.81
0.518.62 ± 1.4913.175.45 ± 1.49
1.015.83 ± 1.1914.281.55 ± 1.19