表6 体外测试中,不同溶液中添加蛋白质对医用金属材料腐蚀速率的影响
Table 6 The effects of BSA on the in vitro corrosion rate of biomedical metals in different solutions
MaterialNaClNaCl+NaFNaCl+H2O2PBSHBSSSBFRinger??sSBPM199DMEM
Mg?????T?
Mg-Ca??
AZ31??
AZ80?
AZ91????
M1AT
LAE442??
ZK21-0.2Sc??
Mg-Nd-Zn-Zr??
WE43??
MgY??
Mg-Zn-Zr??
Zn??
316L stainless steel???????

Low carbon austenite

stainless steel

??

430/304

stainless steel

??
Ti??????
Ti-6Al-4V???????
CoCrMo???
NbT