| 表2 典型高强度不锈钢的力学性能[13,14,15,16,17,18,19,20,21] |
| Table 2 Mechanical properties of typical high strength stainless steels[13,14,15,16,17,18,19,20,21] |
|
| Steel | Rp0.2 / MPa | Rm / MPa | KIC / (MPa·m1/2) | AKU / J | Strengthening phase |
|---|
| 17-4PH | 1262 | 1365 | - | 21 | Cu | | 15-5PH | 1213 | 1289 | - | 79 | Cu | | Custom450 | 1269 | 1289 | - | 55 | Cu | | PH13-8 | 1448 | 1551 | - | 41 | NiAl | | Ultrafort401 | 1565 | 1669 | 103 | 56 | Ni3Ti | | Ultrafort403 | 1669 | 1689 | 60 | 34 | Ni3Ti | | 1RK91 | 1500 | 1700 | 58 | 27 | Cu/Ni3Ti | | Custom465 | 1703 | 1779 | 71 | - | Ni3Ti | | USS122G | 1550 | 1940 | 90 | - | Laves/α' | | Ferrium?S53 | 1551 | 1986 | 77 | - | M2C |
|
|
|