超高强高韧化钢的研究进展和展望
|
|
罗海文,沈国慧
|
Progress and Perspective of Ultra-High Strength Steels Having High Toughness
|
|
Haiwen LUO,Guohui SHEN
|
|
| 表4 典型马氏体时效超高强韧钢的力学性能[18,21,22,23,24,25] |
| Table 4 Mechanical properties of typical ultra-high strength maraging steels[18,21,22,23,24,25] |
|
| Steel | YS / MPa | UTS / MPa | EL / % | Hardness / HB | Ak (20 ℃) / J | Ref. |
|---|
| 18Ni3Al4Mo | 1947 | 2197 | 8.2 | - | - | [18] | | 18Ni(250) | 1819 | 1854 | 12.19 | 481 | 35 | [21] | | T250 | 1500 | 1860 | 11.5 | 481 | 58 | [22] | | W250 | 1780 | 1800 | 9 | - | 25 | [23] | | 15Ni6Mo4Cu1Ti | 1785 | 1893 | 9.5 | 525 | 30 | [24] | | 14Ni3Cr3Mo1.5Ti | 1750 | 1820 | 13.5 | 496 | - | [25] |
|
|
|