| 表2 主要低合金超高强韧钢的力学性能[11,14,30,32,36,37,38,39,40] |
| Table 2 Mechanical properties of typical low alloyed ultra-high strength steels[11,14,30,32,36,37,38,39,40] |
|
| Steel | YS / MPa | UTS / MPa | EL / % | Hardness / HB | Ak (20 ℃) / J | Ref. |
|---|
| HY130-1 | 896 | 970 | 23 | - | - | [11] | | 4340 | 1627 | 1792 | 8.6 | 536 | - | [14] | | 4140 | 1025 | 1100 | 11 | 320 | 40 | [30] | | 4130 | 880 | 980 | - | - | 16 | [32] | | 300M | 1705 | 1930 | 10 | 595 | 20 | [36] | | 30CrMnSiNi2A | 1400 | 1720 | 10 | - | 75 | [37] | | 45CrNiMo1VA | 1780 | 2000 | 8 | 543 | 31 | [38] | | 35Si2Mn2MoVA | 1550 | 1850 | 11 | - | 55 | [39] | | 406 | 1700 | 2000 | 11 | - | 50 | [40] |
|
|
|