一般大气环境下锈蚀结构钢表面特征与随机模型
|
|
王友德,徐善华,李晗,张海江
|
Surface Characteristics and Stochastic Model of Corroded Structural Steel Under General Atmospheric Environment
|
|
Youde WANG,Shanhua XU,Han LI,Haijiang ZHANG
|
|
| 表1 试件腐蚀程度参数 |
| Table 1 Corrosion degree parameters of steel plates |
|
| Corrosion condition | Sample No. | Corrosion time | T0 / mm | Tmax / mm | γ / % | Δte / μm |
|---|
| Accelerated corrosion | A1 | 40 d | 7.2 | 7.20 | 2.76 | 199 | | A2 | 80 d | 7.2 | 7.20 | 4.26 | 307 | | A3 | 120 d | 7.2 | 7.14 | 6.04 | 435 | | A4 | 160 d | 7.2 | 7.06 | 8.72 | 628 | | A5 | 240 d | 7.2 | 7.03 | 9.07 | 653 | | A6 | 320 d | 7.2 | 6.82 | 12.56 | 904 | | Natural corrosion | HTF | 8 a | 9.0 | 7.98 | 21.18 | 1906 | | HBF | 8 a | 9.0 | 7.93 | 21.85 | 1966 | | HW | 8 a | 6.5 | 5.28 | 29.92 | 1944 | | STF | 8 a | 9.0 | 7.84 | 21.97 | 1977 | | SBF | 8 a | 9.0 | 7.80 | 22.64 | 2037 | | SW | 8 a | 6.5 | 5.27 | 32.99 | 2144 | | VTF | 8 a | 8.0 | 7.36 | 16.94 | 1355 | | VBF | 8 a | 8.0 | 7.25 | 19.21 | 1537 | | VW | 8 a | 6.0 | 5.42 | 19.73 | 1184 |
|
|
|