| (atomic fraction / %) | mm | K | K | HV |
| [B-B2Fe8]Fe | Fe75B25 | <1.0 | - | 712 | - |
| [(B0.4Si0.6)-B2Fe8]Fe (y=0.6) | Fe75B20Si5 | <1.0 | - | 825 | - |
| [(B0.2Si0.8)-B2Fe8]Fe (y=0.8) | Fe75B18.33Si6.67 | <1.0 | - | 833 | - |
| [Si-B2Fe8]Fe (y=1.0) | Fe75B16.67Si8.33 | <1.0 | - | 839 | - |
| [Si-B1.8Si0.2Fe8]Fe (y=1.2) | Fe75B15Si10 | <1.0 | - | 838 | - |
| [Si-B1.6Si0.4Fe8]Fe (y=1.4) | Fe75B13.33Si11.67 | <1.0 | - | 832 | - |
| [Si-B2Fe7.6Y0.4]Fe (RE=Y) | Fe71.67B16.67Si8.33Y3.33 | <1.0 | - | 923 | - |
| [Si-B2Fe7.6Dy0.4]Fe (RE=Dy) | Fe71.67B16.67Si8.33Dy3.33 | <1.0 | - | 924 | - |
| [Si-B2Fe7.6Ce0.4]Fe (RE=Ce) | Fe71.67B16.67Si8.33Ce3.33 | <1.0 | - | 902 | - |
| [Si-B2Fe7.6Nd0.4]Fe (RE=Nd) | Fe71.67B16.67Si8.33Nd3.33 | <1.0 | - | 917 | - |
| [Si-B2Fe7.6Pr0.4]Fe (RE=Pr) | Fe71.67B16.67Si8.33Pr3.33 | <1.0 | - | 914 | - |
| [Si-B2Fe7.6Sm0.4]Fe (RE=Sm) | Fe71.67B16.67Si8.33Sm3.33 | <1.0 | - | 898 | - |
| [Si-B2Fe7.6Gd0.4]Fe (RE=Gd) | Fe71.67B16.67Si8.33Gd3.33 | <1.0 | - | 921 | - |
| (atomic fraction / %) | mm | K | K | HV |
| [Si-B2Fe7.8Zr0.2]Fe (ETM=Zr, z=0.2) | Fe73.33B16.67Si8.33Zr1.67 | 2.0 | 839 | 873 | 1120±9 |
| [Si-B2Fe7.7Zr0.3]Fe (ETM=Zr, z=0.3) | Fe72.50B16.67Si8.33Zr2.50 | 2.5 | 846 | 882 | 1131±7 |
| [Si-B2Fe7.6Zr0.4]Fe (ETM=Zr, z=0.4) | Fe71.67B16.67Si8.33Zr3.33 | 2.5 | 851 | 888 | 1149±7 |
| [Si-B2Fe7.5Zr0.5]Fe (ETM=Zr, z=0.5) | Fe70.83B16.67Si8.33Zr4.17 | 2.0 | 854 | 891 | 1145±8 |
| [Si-B2Fe7.4Zr0.6]Fe (ETM=Zr, z=0.6) | Fe70B16.67Si8.33Zr5 | 1.5 | 868 | 903 | 1156±7 |
| [Si-B2Fe7.3Zr0.7]Fe (ETM=Zr, z=0.7) | Fe69.17B16.67Si8.33Zr5.83 | 1.5 | 875 | 909 | 1170±10 |
| [Si-B2Fe7.2Zr0.8]Fe (ETM=Zr, z=0.8) | Fe68.33B16.67Si8.33Zr6.67 | 1.0 | 878 | 918 | 1184±8 |
| [Si-B2Fe7.1Zr0.9]Fe (ETM=Zr, z=0.9) | Fe67.5B16.67Si8.33Zr7.5 | 1.0 | 890 | 922 | 1195±13 |
| [Si-B2Fe7.0Zr1.0]Fe (ETM=Zr, z=1.0) | Fe66.67B16.67Si8.33Zr8.33 | <1.0 | 895 | 925 | 1197±15 |
| [Si-B2Fe7.8Hf0.2]Fe (ETM=Hf, z=0.2) | Fe73.33B16.67Si8.33Hf1.67 | 1.0 | 840 | 872 | 1115±13 |
| [Si-B2Fe7.7Hf0.3]Fe (ETM=Hf, z=0.3) | Fe72.50B16.67Si8.33Hf2.50 | 2.5 | 852 | 885 | 1121±19 |
| [Si-B2Fe7.6Hf0.4]Fe (ETM=Hf, z=0.4) | Fe71.67B16.67Si8.33Hf3.33 | 2.0 | 854 | 887 | 1153±8 |
| [Si-B2Fe7.5Hf0.5]Fe (ETM=Hf, z=0.5) | Fe70.83B16.67Si8.33Hf4.17 | 1.5 | 858 | 893 | 1138±9 |
| [Si-B2Fe7.4Hf0.6]Fe (ETM=Hf, z=0.6) | Fe70B16.67Si8.33Hf5 | 1.0 | 861 | 901 | 1168±8 |
| [Si-B2Fe7.3Hf0.7]Fe (ETM=Hf, z=0.7) | Fe69.17B16.67Si8.33Hf5.83 | 1.0 | 870 | 908 | 1174±9 |
| [Si-B2Fe7.2Hf0.8]Fe (ETM=Hf, z=0.8) | Fe68.33B16.67Si8.33Hf6.67 | <1.0 | 876 | 911 | - |
| [Si-B2Fe7.1Hf0.9]Fe (ETM=Hf, z=0.9) | Fe67.5B16.67Si8.33Hf7.5 | <1.0 | 886 | 918 | - |
| [Si-B2Fe7.8Nb0.2]Fe (ETM=Nb, z=0.2) | Fe73.33B16.67Si8.33Nb1.67 | 1.0 | - | 861 | 1087±12 |
| [Si-B2Fe7.7Nb0.3]Fe (ETM=Nb, z=0.3) | Fe72.5B16.67Si8.33Nb2.5 | 2.0 | 835 | 869 | 1090±1 |
| [Si-B2Fe7.6Nb0.4]Fe (ETM=Nb, z=0.4) | Fe71.67B16.67Si8.33Nb3.33 | 2.5 | 843 | 873 | 1108±11 |
| [Si-B2Fe7.5Nb0.5]Fe (ETM=Nb, z=0.5) | Fe70.83B16.67Si8.33Nb4.17 | 2.5 | 845 | 881 | 1113±4 |
| [Si-B2Fe7.4Nb0.6]Fe (ETM=Nb, z=0.6) | Fe70B16.67Si8.33Nb5 | 2.0 | 853 | 885 | 1126±9 |
| [Si-B2Fe7.3Nb0.7]Fe (ETM=Nb, z=0.7) | Fe69.17B16.67Si8.33Nb5.83 | 1.5 | 854 | 895 | 1150±13 |
| [Si-B2Fe7.2Nb0.8]Fe (ETM=Nb, z=0.8) | Fe68.33B16.67Si8.33Nb6.67 | 1.5 | 856 | 902 | 1172±20 |
| [Si-B2Fe7.1Nb0.9]Fe (ETM=Nb, z=0.9) | Fe67.5B16.67Si8.33Nb7.5 | 1.5 | 862 | 911 | 1173±25 |
| [Si-B2Fe7.0Nb1.0]Fe (ETM=Nb, z=1.0) | Fe66.67B16.67Si8.33Nb8.33 | 1.5 | 875 | 917 | 1188±28 |
| [Si-B2Fe6.8Nb1.2]Fe (ETM=Nb, z=1.2) | Fe65B16.67Si8.33Nb10 | 1.0 | 889 | 930 | - |
| [Si-B2Fe7.8Ta0.2]Fe (ETM=Ta, z=0.2) | Fe73.33B16.67Si8.33Ta1.67 | <1.0 | - | 858 | - |
| [Si-B2Fe7.7Ta0.3]Fe (ETM=Ta, z=0.3) | Fe72.5B16.67Si8.33Ta2.5 | <1.0 | - | 865 | - |
| [Si-B2Fe7.6Ta0.4]Fe (ETM=Ta, z=0.4) | Fe71.67B16.67Si8.33Ta3.33 | 1.0 | 843 | 873 | 1117±6 |
| [Si-B2Fe7.5Ta0.5]Fe (ETM=Ta, z=0.5) | Fe70.83B16.67Si8.33Ta4.17 | 1.0 | 850 | 884 | 1130±10 |
| [Si-B2Fe7.4Ta0.6]Fe (ETM=Ta, z=0.6) | Fe70B16.67Si8.33Ta5 | 1.0 | 856 | 889 | 1143±10 |
| [Si-B2Fe7.3Ta0.7]Fe (ETM=Ta, z=0.7) | Fe69.16B16.67Si8.33Ta5.83 | 1.0 | 856 | 891 | 1154±11 |
| [Si-B2Fe7.2Ta0.8]Fe (ETM=Ta, z=0.8) | Fe68.33B16.67Si8.33Ta6.67 | <1.0 | 859 | 896 | - |
| [Si-B2Fe7.1Ta0.9]Fe (ETM=Ta, z=0.9) | Fe67.5B16.67Si8.33Ta7.5 | <1.0 | 863 | 910 | - |
| [Si-B2Fe7.0Ta1.0]Fe (ETM=Ta, z=1.0) | Fe66.67B16.67Si8.33Ta8.33 | <1.0 | 874 | 913 | - |