Ti2AlNb异形粉末环件的轧制成形与性能研究
卢正冠,吴杰,徐磊,崔潇潇,杨锐

Ring Rolling Forming and Properties of Ti2AlNb Special Shaped Ring Prepared by Powder Metallurgy
Zhengguan LU,Jie WU,Lei XU,Xiaoxiao CUI,Rui YANG
表3 Ti2AlNb粉末合金与铸锭变形合金在不同变形条件下的峰值应力
Table 3 Peak stresses of Ti2AlNb PM alloy and wrought alloy under different deformation conditions
TemperatureTypeStrain rate / s-1
℃0.0010.010.11
930HIP143248363562
Wrought146288353603
980HIP60168212255
Wrought49172182222
1005HIP59141245310
Wrought54149251337
1030HIP4690102147
Wrought439595154
1050HIP3180160201
Wrought31103153223