表2 L18(37) 正交实验及CuSO4溶液点滴实验结果
Table 2 L18(37) orthogonal experiments and CuSO4 drip time
Test No. H3PO4
mL/L
ZnO
g/L
KClO3
g/L
Zn(H2PO4)2
g/L
C4H6O6
g/L
Zn(NO3)2
g/L
OP-10
g/L
CuSO4intravenous drip time / s
1 300 10 3 8 6 3 8 77
2 300 12 4 9 8 4 10 62
3 300 14 5 10 10 5 12 125
4 310 10 3 9 8 5 12 68
5 310 12 4 10 10 3 8 75
6 310 14 5 8 6 4 10 128
7 320 10 4 8 10 4 12 176
8 320 12 5 9 6 5 8 87
9 320 14 3 10 8 3 10 169
10 300 10 5 10 8 4 8 85
11 300 12 3 8 10 5 10 92
12 300 14 4 9 6 3 12 78
13 310 10 4 10 6 5 10 158
14 310 12 5 8 8 3 12 98
15 310 14 3 9 10 4 8 89
16 320 10 5 9 10 3 10 82
17 320 12 3 10 6 4 12 63
18 320 14 4 8 8 5 8 56