20SiMn钢在恒定pH值的碳酸盐溶液中的腐蚀行为*
|
|
曹凤婷, 魏洁, 董俊华, 柯伟
|
CORROSION BEHAVIOR OF 20SiMn STEEL REBAR IN CARBONATE/BICARBONATE SOLUTIONS WITH THE SAME pH VALUE
|
|
CAO Fengting, WEI Jie, DONG Junhua, KE Wei
|
|
| 表4 0.5 mol/L 碳酸盐缓冲液中的EIS 拟合结果 |
| Table 4 EIS fitting results of the parameters in 0.5 mol/L carbonate buffer solution |
|
Immerse time d | Rs Ω·cm2 | Q1 Ω-1·cm-2·sn | n1 | R1 Ω·cm2 | Qct Ω-1·cm-2·sn | nct | Rct Ω·cm2 | | 1 | 3.222 | 2.339×10-4 | 0.8779 | 57790 | 9.592×10-5 | 0.9111 | 3975 | | 2 | 4.804 | 2.320×10-4 | 0.8754 | 66880 | 9.332×10-5 | 0.9016 | 5297 | | 3 | 5.499 | 2.218×10-4 | 0.8802 | 72840 | 9.025×10-5 | 0.9006 | 6201 | | 4 | 3.539 | 2.133×10-4 | 0.8883 | 75630 | 8.630×10-5 | 0.9058 | 6585 | | 5 | 10.86 | 8.927×10-5 | 0.9358 | 2.946×105 | 1.225×10-4 | 0.9140 | 1.310×104 | | 6 | 10.53 | 7.277×10-5 | 0.9365 | 4.733×105 | 1.384×10-4 | 0.9088 | 1.257×104 | | 7 | 10.03 | 7.713×10-5 | 0.9354 | 4.102×105 | 1.335×10-4 | 0.9146 | 1.270×104 |
|
|
|