温度对国产核级316L不锈钢在加Zn水中电化学腐蚀性能的影响*
|
|
刘侠和, 吴欣强, 韩恩厚
|
EFFECTS OF TEMPERATURE ON LECTROCHEMICAL CORROSION OF DOMESTIC NUCLEAR-GRADE 316L STAINLESS STEEL IN Zn-INJECTED AQUEOUS ENVIRONMENT
|
|
LIU Xiahe, WU Xinqiang, HAN En-hou
|
|
| |
| 表2 316L SS在323.15~603.15 K, B+Li加Zn水中氧化膜EIS等效电路的拟合结果 |
|
| T / K | Rs / 102 Ω | C1 / 10-7 | n1 | R1 / 102 Ω | C2 / 10-5 | n2 | R2 / 104 Ω | | 323.15 | 11.43 | 756.74 | 0.686 | 0.04 | 13.90 | 0.876 | 8.23 | | 423.15 | 2.51 | 678.73 | 0.524 | 0.01 | 14.51 | 0.850 | 7.51 | | 473.15 | 2.31 | 56.82 | 0.621 | 9.18 | 18.33 | 0.974 | 5.25 | | 523.15 | 1.05 | 8.99 | 0.737 | 5.68 | 34.39 | 0.905 | 2.75 | | 573.15 | 0.89 | 6.67 | 0.642 | 4.65 | 66.34 | 0.817 | 0.18 | | 603.15 | 0.76 | 5.56 | 0.678 | 3.95 | 79.32 | 0.976 | 0.14 |
|
|
|