温度对国产核级316L不锈钢在加Zn水中电化学腐蚀性能的影响*
|
|
刘侠和, 吴欣强, 韩恩厚
|
EFFECTS OF TEMPERATURE ON LECTROCHEMICAL CORROSION OF DOMESTIC NUCLEAR-GRADE 316L STAINLESS STEEL IN Zn-INJECTED AQUEOUS ENVIRONMENT
|
|
LIU Xiahe, WU Xinqiang, HAN En-hou
|
|
| |
| 表1 316L SS在323.15~603.15 K, B+Li水环境中氧化膜EIS等效电路的拟合结果 |
|
| T / K | Rs / 102 Ω | C1 / 10-7 | n1 | R1 / 102 Ω | C2 / 10-5 | n2 | R2 / 104 Ω | | 323.15 | 12.61 | 654.73 | 0.657 | 0.05 | 11.35 | 0.988 | 7.66 | | 423.15 | 5.63 | 550.87 | 0.781 | 0.01 | 12.96 | 0.970 | 6.04 | | 473.15 | 2.43 | 87.76 | 0.571 | 8.24 | 16.22 | 0.952 | 4.77 | | 523.15 | 2.08 | 25.97 | 0.555 | 5.96 | 22.58 | 0.736 | 1.98 | | 573.15 | 1.01 | 13.86 | 0.597 | 4.50 | 59.32 | 0.597 | 0.14 | | 603.15 | 0.91 | 9.31 | 0.470 | 3.58 | 76.45 | 0.597 | 0.11 |
|
|
|