NZ30K镁合金时效析出动力学与强化模型的研究*
|
|
王小娜, 韩利战, 顾剑锋
|
PRECIPITATION KINETICS AND YIELD STRENGTH MODEL FOR NZ30K-Mg ALLOY
|
|
WANG Xiaona, HAN Lizhan, GU Jianfeng
|
|
| 表1 NZ30K镁合金等温时效处理后试样的相对析出体积分数和屈服强度 |
| Table 1 The relative precipitation volume fraction and yield strength of NZ30K-Mg alloy isothermally aged with different conditions ( σy —yield strength) |
|
| Specimen No. | T / ℃ | t / h | / % | / MPa | | 1 | 180 | 1 | 0.111 | 109.71 | | 2 | 180 | 2 | 0.174 | 111.43 | | 3 | 180 | 5 | 0.269 | 122.25 | | 4 | 180 | 10 | 0.332 | 125.68 | | 5 | 180 | 20 | 0.397 | 131.29 | | 6 | 180 | 50 | 0.513 | 133.39 | | 7 | 180 | 100 | 0.684 | 141.19 | | 8 | 180 | 200 | 0.897 | 148.88 | | 9 | 200 | 1 | 0.197 | 127.43 | | 10 | 200 | 2 | 0.282 | 135.24 | | 11 | 200 | 5 | 0.397 | 138.00 | | 12 | 200 | 10 | 0.504 | 144.44 | | 13 | 200 | 20 | 0.697 | 148.50 | | 14 | 200 | 50 | 0.941 | 151.53 | | 15 | 250 | 0.25 | 0.304 | 138.28 | | 16 | 250 | 0.5 | 0.548 | 148.89 | | 17 | 250 | 0.75 | 0.717 | 149.60 | | 18 | 250 | 1 | 0.850 | 152.59 |
|
|
|